AA Standards Grade 6063 T831

View suppliers (160)
Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 6063 is an architectural alloy that offers users a high resistance to corrosion and excellent finishing characteristics. Easy to extrude with fair machinability, AA 6063 can be both hot and cold formed and is commonly available as T6 temper as well as T4 temper.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com,ASM Handbook Volume 2 Properties and Selection: Nonferrous Alloys and Special-Purpose Materials.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T831

AA Standards, ASTM B210, ASTM B483

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T831

Mechanical

PropertyValueConditionRelated StandardsComment

Compressive modulus

69.7 MPa

Show Material materials with Compressive modulus of 69.7 MPa

T831

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

T831

AA Standards, ASTM B210, ASTM B483

69 GPa

Show Material materials with Elastic modulus of 69 GPa

T831

Elongation

7.9 %

Show Material materials with Elongation of 7.9 %

T831

10 %

Show Material materials with Elongation of 10 %

T831

Hardness, Brinell

70.0 [-]

Show Material materials with Hardness, Brinell of 70.0 [-]

T831

500 kg load, 10 mm ball

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 6000 Series Aluminium

Shear strength

124.0 MPa

Show Material materials with Shear strength of 124.0 MPa

T831

Tensile strength

195.0 MPa

Show Material materials with Tensile strength of 195.0 MPa

T831

AA Standards, ASTM B210, ASTM B483

205 MPa

Show Material materials with Tensile strength of 205 MPa

T831

210.0 MPa

Show Material materials with Tensile strength of 210.0 MPa

T831

Yield strength

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

T831

AA Standards, ASTM B210, ASTM B483

RP02

185 MPa

Show Material materials with Yield strength of 185 MPa

T831

RP02

190.0 MPa

Show Material materials with Yield strength of 190.0 MPa

T831

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T831

20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T831

AA Standards, ASTM B210, ASTM B483

100 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T831

AA Standards, ASTM B210, ASTM B483

Melting point

615.0 - 655.0 °C

Show Material materials with Melting point of 615.0 - 655.0 °C

T831

AA Standards, ASTM B210, ASTM B483

620.0 °C

Show Material materials with Melting point of 620.0 °C

T831

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

T831

Thermal conductivity

193.0 - 218.0 W/(m·K)

Show Material materials with Thermal conductivity of 193.0 - 218.0 W/(m·K)

T831

AA Standards, ASTM B210, ASTM B483

200.0 W/(m·K)

Show Material materials with Thermal conductivity of 200.0 W/(m·K)

T831

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

29000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 29000000.0 - 34000000.0 S/m

T831

AA Standards, ASTM B210, ASTM B483

Electrical resistivity

2.94e-08 - 3.45e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.45e-08 Ω·m

T831

AA Standards, ASTM B210, ASTM B483

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

97.5 - 99.4 %

Show Material materials with Aluminium of 97.5 - 99.4 %

T831

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T831

AA Standards, ASTM B210, ASTM B483

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T831

AA Standards, ASTM B210, ASTM B483

Iron

0.35 %

Show Material materials with Iron of 0.35 %

T831

AA Standards, ASTM B210, ASTM B483

0.35 %

Show Material materials with Iron of 0.35 %

T831

Magnesium

0.45 - 0.9 %

Show Material materials with Magnesium of 0.45 - 0.9 %

T831

AA Standards, ASTM B210, ASTM B483

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T831

AA Standards, ASTM B210, ASTM B483

Other

0.15 %

Show Material materials with Other of 0.15 %

T831

Silicon

0.2 - 0.6 %

Show Material materials with Silicon of 0.2 - 0.6 %

T831

AA Standards, ASTM B210, ASTM B483

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T831

AA Standards, ASTM B210, ASTM B483

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

T831

AA Standards, ASTM B210, ASTM B483

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832)

Workability

general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832)