All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

2.7 - 2.71 g/cm³

Show Material materials with Density of 2.7 - 2.71 g/cm³

Mechanical

PropertyTemperatureValueComment

Bending Fatigue Strength

23.0 °C

30 MPa

Show Material materials with Bending Fatigue Strength of 30 MPa

Elastic modulus

23.0 °C

69 GPa

Show Material materials with Elastic modulus of 69 GPa

Elongation

23.0 °C

12 - 16 %

Show Material materials with Elongation of 12 - 16 %

Elongation A100

23.0 °C

10 %

Show Material materials with Elongation A100 of 10 %

Elongation A50

23.0 °C

6 - 16 %

Show Material materials with Elongation A50 of 6 - 16 %

Fatigue strength

23.0 °C

28 MPa

Show Material materials with Fatigue strength of 28 MPa

for 5x10⁸ cycles

Hardness, Brinell

23.0 °C

23 - 28 [-]

Show Material materials with Hardness, Brinell of 23 - 28 [-]

500 kg load, 10 mm ball

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

23.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

23.0 °C

25 GPa

Show Material materials with Shear modulus of 25 GPa

Shear strength

23.0 °C

55 MPa

Show Material materials with Shear strength of 55 MPa

Tensile strength

23.0 °C

70 - 110 MPa

Show Material materials with Tensile strength of 70 - 110 MPa

Yield strength

23.0 °C

62 MPa

Show Material materials with Yield strength of 62 MPa

Yield strength Rp0.2

23.0 °C

30 - 75 MPa

Show Material materials with Yield strength Rp0.2 of 30 - 75 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

20.0 °C

2.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K

23.0 °C

2.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.4E-5 1/K

100.0 °C

2.36E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K

Melting point

645 - 655 °C

Show Material materials with Melting point of 645 - 655 °C

Specific heat capacity

23.0 °C

900 J/(kg·K)

Show Material materials with Specific heat capacity of 900 J/(kg·K)

Thermal conductivity

23.0 °C

230 - 234 W/(m·K)

Show Material materials with Thermal conductivity of 230 - 234 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

23.0 °C

3.50E+7 - 3.60E+7 S/m

Show Material materials with Electrical conductivity of 3.50E+7 - 3.60E+7 S/m

Electrical resistivity

23.0 °C

2.78E-8 - 2.86E-8 Ω·m

Show Material materials with Electrical resistivity of 2.78E-8 - 2.86E-8 Ω·m

Chemical properties

PropertyValue

Aluminium

99.6 - 100 %

Show Material materials with Aluminium of 99.6 - 100 %

Copper

0 - 0.05 %

Show Material materials with Copper of 0 - 0.05 %

Iron

0 - 0.35 %

Show Material materials with Iron of 0 - 0.35 %

Magnesium

0 - 0.03 %

Show Material materials with Magnesium of 0 - 0.03 %

Manganese

0 - 0.03 %

Show Material materials with Manganese of 0 - 0.03 %

Other

each 0.03

Silicon

0 - 0.25 %

Show Material materials with Silicon of 0 - 0.25 %

Titanium

0 - 0.03 %

Show Material materials with Titanium of 0 - 0.03 %

Vanadium

0 - 0.05 %

Show Material materials with Vanadium of 0 - 0.05 %

Zinc

0 - 0.05 %

Show Material materials with Zinc of 0 - 0.05 %

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12), poor (H14, H16, H18)

Workability

general (condition): good (O, H12, H14), acceptable (H16, H18)