AA 7075 T6

Want to keep this datasheet? Save it now in your required format

Primary standard name

This material data has been provided by MakeItFrom.com and AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

3.1 g/cm³

Show Material materials with Density of 3.1 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

72 GPa

Show Material materials with Elastic modulus of 72 GPa

Elongation

20.0 °C

6.8 %

Show Material materials with Elongation of 6.8 %

Elongation A50

20.0 °C

2 - 11 %

Show Material materials with Elongation A50 of 2 - 11 %

Hardness, Brinell

20.0 °C

150 [-]

Show Material materials with Hardness, Brinell of 150 [-]

Tensile strength

20.0 °C

450 - 570 MPa

Show Material materials with Tensile strength of 450 - 570 MPa

Yield strength

20.0 °C

470 MPa

Show Material materials with Yield strength of 470 MPa

Yield strength Rp0.2

20.0 °C

380 - 505 MPa

Show Material materials with Yield strength Rp0.2 of 380 - 505 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

20.0 °C

2.3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.3E-5 1/K

Melting point

480 °C

Show Material materials with Melting point of 480 °C

Specific heat capacity

20.0 °C

910 J/(kg·K)

Show Material materials with Specific heat capacity of 910 J/(kg·K)

Thermal conductivity

20.0 °C

130 W/(m·K)

Show Material materials with Thermal conductivity of 130 W/(m·K)

Chemical properties

PropertyValue

Aluminium

86.9 - 91.4 %

Show Material materials with Aluminium of 86.9 - 91.4 %

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

Copper

1.2 - 2 %

Show Material materials with Copper of 1.2 - 2 %

Iron

0.5 %

Show Material materials with Iron of 0.5 %

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

Other

0.15 %

Show Material materials with Other of 0.15 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

Zirconium

0.25 %

Show Material materials with Zirconium of 0.25 %