AA 7075 is a high-strength alloy that offers good stress-corrosion cracking resistance. Known as a mainstay in the aerospace industry since it was introduced, Aluminum 7075 brings moderate toughness as well as an excellent strength-to-weight ratio. It is also important to note that at sub-zero temperatures Aluminum 7075 increases in strength.

Equivalent Materials

This material data has been provided by MakeItFrom.com.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueCondition

Density

3.1 g/cm³

Show Material materials with Density of 3.1 g/cm³

T7

Mechanical

PropertyValueConditionComment

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T7

Elongation

9.3 %

Show Material materials with Elongation of 9.3 %

T7

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

26.4 - 27.1 GPa

Show Material materials with Shear modulus of 26.4 - 27.1 GPa

Typical for Wrought 7000 Series Aluminium

Tensile strength

510.0 MPa

Show Material materials with Tensile strength of 510.0 MPa

T7

Yield strength

410.0 MPa

Show Material materials with Yield strength of 410.0 MPa

T7

Thermal

PropertyValueCondition

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T7

Melting point

480.0 °C

Show Material materials with Melting point of 480.0 °C

T7

Specific heat capacity

910.0 J/(kg·K)

Show Material materials with Specific heat capacity of 910.0 J/(kg·K)

T7

Thermal conductivity

130.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 W/(m·K)

T7

Electrical

PropertyValueComment

Electrical conductivity

18000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 18000000.0 - 34000000.0 S/m

Typical for Wrought 7000 Series Aluminium

Electrical resistivity

2.9e-08 - 5.6e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 - 5.6e-08 Ω·m

Typical for Wrought 7000 Series Aluminium

Chemical properties

PropertyValueCondition

Aluminium

86.9 - 91.4 %

Show Material materials with Aluminium of 86.9 - 91.4 %

T7

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

T7

Copper

1.2 - 2.0 %

Show Material materials with Copper of 1.2 - 2.0 %

T7

Iron

0.5 %

Show Material materials with Iron of 0.5 %

T7

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

T7

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

T7

Other

0.15 %

Show Material materials with Other of 0.15 %

T7

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

T7

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

T7

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

T7

Zirconium

0.25 %

Show Material materials with Zirconium of 0.25 %

T7

Technological properties

Property
Brazing

Excellent

Looking for suppliers of this material? Click to see 128 supplier of AA 7075 T7 on Matmatch