See where AA Standards Grade 1060 H26 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.
Density
ρ2.7 - 2.71 g/cm³ at 23 °C
Dimensions
Dicke
Coefficient of thermal expansion
α2.36E-5 1/K at 20 °C
Melting point
Tm645 - 655 °C
Specific heat capacity
cp900 J/(kg·K) at 23 °C
Thermal conductivity
λ230 - 234 W/(m·K) at 23 °C
Electrical conductivity
σel3.50E+7 - 3.60E+7 S/m at 23 °C
Electrical resistivity
ρel2.78E-8 - 2.86E-8 Ω·m at 23 °C
Element
Weight %
Comment
-
each 0.03
99.6 - 100 %
0 - 0.05 %
0 - 0.35 %
0 - 0.03 %
Brazing
general: possible with commercial processes and methods
Corrosion properties
Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere
General machinability
General: not suitable (O, H12), poor (H14, H16, H18)
Workability
general (condition): good (O, H12, H14), acceptable (H16, H18)