Description

AA 2014 is an alloy with strength, machinability and welding capabilities, Aluminum Alloy AA 2014 is an excellent option. It is a precipitation hardening alloy that maintains strength after heat treatment.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,MakeItFrom.com.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T6510

AA Standards, ASTM B241

3.0 g/cm³

Show Material materials with Density of 3.0 g/cm³

T6510

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T6510

AA Standards, ASTM B241

Elongation

5.0 %

Show Material materials with Elongation of 5.0 %

T6510

AA Standards, ASTM B241

A100

6.0 %

Show Material materials with Elongation of 6.0 %

T6510

AA Standards, ASTM B241

A100

6.1 %

Show Material materials with Elongation of 6.1 %

T6510

7.0 %

Show Material materials with Elongation of 7.0 %

T6510

AA Standards, ASTM B241

A50

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

26.0 - 27.5 GPa

Show Material materials with Shear modulus of 26.0 - 27.5 GPa

Typical for Wrought 2000 Series Aluminium

Tensile strength

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6510

AA Standards, ASTM B241

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6510

AA Standards, ASTM B241

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T6510

AA Standards, ASTM B241

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T6510

Yield strength

365.0 MPa

Show Material materials with Yield strength of 365.0 MPa

T6510

AA Standards, ASTM B241

RP02

400.0 MPa

Show Material materials with Yield strength of 400.0 MPa

T6510

AA Standards, ASTM B241

RP02

410.0 MPa

Show Material materials with Yield strength of 410.0 MPa

T6510

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6510

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6510

AA Standards, ASTM B241

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6510

AA Standards, ASTM B241

Melting point

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T6510

AA Standards, ASTM B241

510.0 °C

Show Material materials with Melting point of 510.0 °C

T6510

Specific heat capacity

870.0 J/(kg·K)

Show Material materials with Specific heat capacity of 870.0 J/(kg·K)

T6510

Thermal conductivity

134.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K)

T6510

AA Standards, ASTM B241

150.0 W/(m·K)

Show Material materials with Thermal conductivity of 150.0 W/(m·K)

T6510

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

20000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m

T6510

AA Standards, ASTM B241

Electrical resistivity

3.45e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m

T6510

AA Standards, ASTM B241

Chemical properties

PropertyValueConditionRelated Standards

Aluminium

90.4 - 95.0 %

Show Material materials with Aluminium of 90.4 - 95.0 %

T6510

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T6510

AA Standards, ASTM B241

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T6510

AA Standards, ASTM B241

Iron

0.70 %

Show Material materials with Iron of 0.70 %

T6510

AA Standards, ASTM B241

0.7 %

Show Material materials with Iron of 0.7 %

T6510

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T6510

AA Standards, ASTM B241

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T6510

AA Standards, ASTM B241

Other

0.15 %

Show Material materials with Other of 0.15 %

T6510

Silicon

0.5 - 1.2 %

Show Material materials with Silicon of 0.5 - 1.2 %

T6510

AA Standards, ASTM B241

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T6510

AA Standards, ASTM B241

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T6510

AA Standards, ASTM B241

Zirconium

0.2 %

Show Material materials with Zirconium of 0.2 %

T6510

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: sufficient, in principle it should be protected

General machinability

General: poor (O), good to acceptable

Workability

general (condition): poor(T3, T4, T451), not suitable (T6, T651, T6510, T6511)