General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H22 | EN 573-3, EN 485, EN 546, EN 683 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 180° | 0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | H22 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | H22 | EN 573-3, EN 485 | ||||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H22 | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H22 | EN 573-3, EN 485 | ||||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastic modulus of 60.0 - 65.0 GPa | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongation | 2.0 % Show Material materials with Elongation of 2.0 % | H22 | EN 573-3, EN 546 | A50 | ||
4.0 % Show Material materials with Elongation of 4.0 % | H22 | EN 573-3, EN 485, EN 546 | A50 | |||
5.0 % Show Material materials with Elongation of 5.0 % | H22 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | A50 | |||
7.0 % Show Material materials with Elongation of 7.0 % | H22 | EN 573-3, EN 546, EN 683 | A50 | |||
8.0 % Show Material materials with Elongation of 8.0 % | H22 | EN 573-3, EN 683 | A50 | |||
10.0 % Show Material materials with Elongation of 10.0 % | H22 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 30.0 [-] Show Material materials with Hardness, Brinell of 30.0 [-] | H22 | EN 573-3, EN 485 | |||
20.0 °C | 32.0 [-] Show Material materials with Hardness, Brinell of 32.0 [-] | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Shear modulus of 24.0 - 26.0 GPa | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Tensile strength | 90.0 - 135.0 MPa Show Material materials with Tensile strength of 90.0 - 135.0 MPa | H22 | EN 573-3, EN 546, EN 683 | |||
95.0 - 135.0 MPa Show Material materials with Tensile strength of 95.0 - 135.0 MPa | H22 | EN 573-3, EN 485 | ||||
20.0 °C | 100.0 - 140.0 MPa Show Material materials with Tensile strength of 100.0 - 140.0 MPa | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | ||
20 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | ||
20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683, DIN 1712-3, EN 573-4 | Sheet, Strip | ||
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
200.0 °C | 2.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
300.0 °C | 2.54e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Melting point | 644.0 - 657.0 °C Show Material materials with Melting point of 644.0 - 657.0 °C | H22 | EN 573-3, EN 485, EN 546, EN 683 | |||
Specific heat capacity | 900.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Thermal conductivity | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K) | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 33000000.0 - 34000000.0 S/m Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m | H22 | EN 573-3, EN 485, EN 546, EN 683 | ||
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m | H22 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
Electrical resistivity | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m | H22 | EN 573-3, EN 485, EN 546, EN 683 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Manganese | 0.05 % Show Material materials with Manganese of 0.05 % | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H22 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |