General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 65.0 MPa Show Material materials with Bending Fatigue Strength of 65.0 MPa | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
Bending angle 90° | 1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H18 | EN 573-3, EN 485 | |||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H18 | EN 573-3, EN 485 | ||||
3.0 °/t Show Material materials with Bending angle 90° of 3.0 °/t | H18 | EN 573-3, EN 485 | ||||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastic modulus of 60.0 - 65.0 GPa | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
Elongation | 1.0 % Show Material materials with Elongation of 1.0 % | H18 | EN 573-3, EN 485, EN 546, EN 683 | A50 | ||
2.0 % Show Material materials with Elongation of 2.0 % | H18 | EN 573-3, EN 485 | A50 | |||
3.0 % Show Material materials with Elongation of 3.0 % | H18 | EN 573-3, EN 754 | A100 | |||
3.0 % Show Material materials with Elongation of 3.0 % | H18 | EN 573-3, EN 754 | A50 | |||
20.0 °C | 1.0 % Show Material materials with Elongation of 1.0 % | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube, Wire | A10 | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | H18 | EN 573-3, EN 485 | |||
20.0 °C | 38.0 [-] Show Material materials with Hardness, Brinell of 38.0 [-] | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Wire | ||
20.0 °C | 42.0 [-] Show Material materials with Hardness, Brinell of 42.0 [-] | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Shear modulus of 24.0 - 26.0 GPa | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
Tensile strength | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | H18 | EN 573-3, EN 546, EN 683 | |||
140.0 - 200.0 MPa Show Material materials with Tensile strength of 140.0 - 200.0 MPa | H18 | EN 573-3, EN 546 | ||||
150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | H18 | EN 573-3, EN 485, EN 754 | ||||
20.0 °C | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Tensile strength of 140.0 - 180.0 MPa | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
20 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
200.0 °C | 2.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
300.0 °C | 2.54e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
Melting point | 644.0 - 657.0 °C Show Material materials with Melting point of 644.0 - 657.0 °C | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |||
Specific heat capacity | 900.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Thermal conductivity | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K) | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 33000000.0 - 34000000.0 S/m Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | ||
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m | H18 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | |
Electrical resistivity | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | H18 | EN 573-3, EN 485, EN 546, EN 683, EN 754 | |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Manganese | 0.05 % Show Material materials with Manganese of 0.05 % | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H18 | DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 546, EN 683, EN 754 | Rod, Sheet, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |