DIN 1712-3 Grade 3.0285 H18

Want to keep this datasheet? Save it now in your required format

Description

Pure aluminium This material is well anodically oxidizable, and possesses a good electrical and thermal conductivity. The splinter-giving workability is bad because of danger of smearing. Its mechanical strength is low, the plasticity high. The forming capacity and the chemical as well as the weather proofness are excellent. The material is well suitable for welding and braze welding. Application: Apparatus engineering, roll bond, z-bond, household devices, camp and transportation containers for the chemical, pharmaceutical and food industry, roofing, linings, arts and crafts, packing, flow pressed parts (tubes, tube, doses, bottles).

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H18

EN 573-3, EN 1301, EN 485

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H18

EN 573-3, EN 485

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H18

EN 573-3, EN 485

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H18

EN 573-3, EN 485

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-3, EN 1301, EN 485

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Elongation

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 1301

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip, Tube

A10

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Wire

A10

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip, Tube

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod

Hardness, Brinell

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

H18

EN 573-3, EN 485

20.0 °C

30.0 [-]

Show Material materials with Hardness, Brinell of 30.0 [-]

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube, Wire

20.0 °C

36.0 [-]

Show Material materials with Hardness, Brinell of 36.0 [-]

H18

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Tensile strength

120.0 MPa

Show Material materials with Tensile strength of 120.0 MPa

H18

EN 573-3, EN 1301

125.0 MPa

Show Material materials with Tensile strength of 125.0 MPa

H18

EN 573-3, EN 485

20.0 °C

110.0 MPa

Show Material materials with Tensile strength of 110.0 MPa

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

20.0 °C

120.0 - 160.0 MPa

Show Material materials with Tensile strength of 120.0 - 160.0 MPa

H18

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

20.0 °C

120.0 MPa

Show Material materials with Tensile strength of 120.0 MPa

H18

DIN 1712-3, EN 573-3, EN 573-4

Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 485

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 485

Melting point

659.0 °C

Show Material materials with Melting point of 659.0 °C

H18

EN 573-3, EN 1301, EN 485

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Thermal conductivity

225 W/(m·K)

Show Material materials with Thermal conductivity of 225 W/(m·K)

H18

EN 573-3, EN 1301, EN 485

20.0 °C

215.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 W/(m·K)

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34500000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m

H18

EN 573-3, EN 1301, EN 485

20.0 °C

36400000.0 - 37000000.0 S/m

Show Material materials with Electrical conductivity of 36400000.0 - 37000000.0 S/m

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

Electrical resistivity

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m

H18

EN 573-3, EN 1301, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.8 %

Show Material materials with Aluminium of 99.8 %

H18

EN 573-3, EN 1301, EN 485

Copper

0.03 %

Show Material materials with Copper of 0.03 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Iron

0.15 %

Show Material materials with Iron of 0.15 %

H18

DIN 1712-3, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube, Wire

0.15 %

Show Material materials with Iron of 0.15 %

H18

EN 573-3, EN 1301, EN 485

Magnesium

0.02 %

Show Material materials with Magnesium of 0.02 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Manganese

0.02 %

Show Material materials with Manganese of 0.02 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Silicon

0.15 %

Show Material materials with Silicon of 0.15 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Titanium

0.02 %

Show Material materials with Titanium of 0.02 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Zinc

0.06 %

Show Material materials with Zinc of 0.06 %

H18

DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485

Rod, Sheet, Strip, Tube, Wire

Technological properties

Property
Anodizing

decorative: very good, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)