General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.73 g/cm³ Show Material materials with Density of 2.73 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 2.73 g/cm³ Show Material materials with Density of 2.73 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
Bending angle 180° | 1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | O | EN 573-3, EN 485 | |||
Bending angle 90° | 1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | O | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | O | EN 573-3, EN 485 | ||||
Elastic modulus | 69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastic modulus of 60.0 - 65.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | ||
Elongation | -196.0 °C | 46.0 % Show Material materials with Elongation of 46.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | ||
-80.0 °C | 42.0 % Show Material materials with Elongation of 42.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
-20.0 °C | 41.0 % Show Material materials with Elongation of 41.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
7.0 % Show Material materials with Elongation of 7.0 % | O | EN 573-3, EN 546 | A50 | |||
8.0 % Show Material materials with Elongation of 8.0 % | O | EN 573-3, EN 546 | A50 | |||
12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
15.0 % Show Material materials with Elongation of 15.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
17.0 % Show Material materials with Elongation of 17.0 % | O | EN 573-3, EN 485 | A50 | |||
18.0 % Show Material materials with Elongation of 18.0 % | O | EN 573-3, EN 683 | A50 | |||
19.0 % Show Material materials with Elongation of 19.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 % Show Material materials with Elongation of 20.0 % | O | EN 573-3, EN 754, EN 755 | A50 | |||
21.0 % Show Material materials with Elongation of 21.0 % | O | EN 573-3, EN 485 | A50 | |||
24.0 % Show Material materials with Elongation of 24.0 % | O | EN 573-3, EN 485 | A50 | |||
25.0 % Show Material materials with Elongation of 25.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | A100 | |||
28.0 % Show Material materials with Elongation of 28.0 % | O | EN 573-3, EN 485 | A50 | |||
35.0 % Show Material materials with Elongation of 35.0 % | O | EN 573-3, EN 1301 | ||||
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Wire | A100 | |
20.0 °C | 19.0 % Show Material materials with Elongation of 19.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod | A10 | |
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Tube, Wire | A10 | |
20.0 °C | 21.0 % Show Material materials with Elongation of 21.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | A10 | |
20.0 °C | 22.0 % Show Material materials with Elongation of 22.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Tube | ||
20.0 °C | 24.0 % Show Material materials with Elongation of 24.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
20.0 °C | 40.0 % Show Material materials with Elongation of 40.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
100.0 °C | 43.0 % Show Material materials with Elongation of 43.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
150.0 °C | 47.0 % Show Material materials with Elongation of 47.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
200.0 °C | 60.0 % Show Material materials with Elongation of 60.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
260.0 °C | 65.0 % Show Material materials with Elongation of 65.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
320.0 °C | 70.0 % Show Material materials with Elongation of 70.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
370.0 °C | 70.0 % Show Material materials with Elongation of 70.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
Hardness, Brinell | 27.0 [-] Show Material materials with Hardness, Brinell of 27.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 25.0 [-] Show Material materials with Hardness, Brinell of 25.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Wire | ||
20.0 °C | 28.0 [-] Show Material materials with Hardness, Brinell of 28.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
20.0 °C | 30.0 [-] Show Material materials with Hardness, Brinell of 30.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Shear modulus of 24.0 - 26.5 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | ||
Tensile strength | -196.0 °C | 232.0 MPa Show Material materials with Tensile strength of 232.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | ||
-80.0 °C | 137.0 MPa Show Material materials with Tensile strength of 137.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
-20.0 °C | 119.0 MPa Show Material materials with Tensile strength of 119.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
80.0 - 130.0 MPa Show Material materials with Tensile strength of 80.0 - 130.0 MPa | O | EN 573-3, EN 546, EN 683 | ||||
90.0 - 130.0 MPa Show Material materials with Tensile strength of 90.0 - 130.0 MPa | O | EN 573-3, EN 485 | ||||
95.0 - 130.0 MPa Show Material materials with Tensile strength of 95.0 - 130.0 MPa | O | EN 573-3, EN 754 | ||||
95.0 - 135.0 MPa Show Material materials with Tensile strength of 95.0 - 135.0 MPa | O | EN 573-3, EN 755 | ||||
130.0 MPa Show Material materials with Tensile strength of 130.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 90.0 - 140.0 MPa Show Material materials with Tensile strength of 90.0 - 140.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
20.0 °C | 95.0 MPa Show Material materials with Tensile strength of 95.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Tube, Wire | ||
20.0 °C | 112.0 MPa Show Material materials with Tensile strength of 112.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
100.0 °C | 91.0 MPa Show Material materials with Tensile strength of 91.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
150.0 °C | 77.0 MPa Show Material materials with Tensile strength of 77.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
200.0 °C | 57.0 MPa Show Material materials with Tensile strength of 57.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
260.0 °C | 47.0 MPa Show Material materials with Tensile strength of 47.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
320.0 °C | 28.0 MPa Show Material materials with Tensile strength of 28.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | |||
370.0 °C | 19.0 MPa Show Material materials with Tensile strength of 19.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Melting point | 645.0 - 655.0 °C Show Material materials with Melting point of 645.0 - 655.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Specific heat capacity | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire | |
Thermal conductivity | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Electrical resistivity | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Electrical resistivity of 3.57e-08 - 4.55e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire |
0.70 % Show Material materials with Iron of 0.70 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Manganese | 0.9 - 1.5 % Show Material materials with Manganese of 0.9 - 1.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Titanium | 0.1 Show Material materials with Titanium of 0.1 | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Rod, Sheet, Strip, Tube, Wire |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |