General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 2.73 g/cm³ Show Material materials with Density of 2.73 g/cm³ | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastic modulus of 60.0 - 65.0 GPa | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | |
Elongation | 20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | A10 |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet | A10 | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet | ||
Hardness, Brinell | 20.0 °C | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet | |
20.0 °C | 55.0 [-] Show Material materials with Hardness, Brinell of 55.0 [-] | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 24.0 - 26.5 GPa Show Material materials with Shear modulus of 24.0 - 26.5 GPa | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | |
Tensile strength | 20.0 °C | 120.0 - 160.0 MPa Show Material materials with Tensile strength of 120.0 - 160.0 MPa | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet | |
20.0 °C | 185.0 MPa Show Material materials with Tensile strength of 185.0 MPa | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.2e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 - 2.4e-05 1/K | Typical for Wrought 3000 Series Aluminium | ||||
Melting point | 629.0 - 654.0 °C Show Material materials with Melting point of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium | ||||
Specific heat capacity | 20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | |
Thermal conductivity | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K) | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip | |
Electrical resistivity | 3.4e-08 - 4.2e-08 Ω·m Show Material materials with Electrical resistivity of 3.4e-08 - 4.2e-08 Ω·m | Typical for Wrought 3000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 Show Material materials with Chromium of 0.1 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Copper | 0.1 Show Material materials with Copper of 0.1 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Iron | 0.7 Show Material materials with Iron of 0.7 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Magnesium | 0.3 Show Material materials with Magnesium of 0.3 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Manganese | 0.9 - 1.5 % Show Material materials with Manganese of 0.9 - 1.5 % | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Silicon | 0.5 Show Material materials with Silicon of 0.5 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Titanium | 0.1 Show Material materials with Titanium of 0.1 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Zinc | 0.2 Show Material materials with Zinc of 0.2 | H1x | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 513, VdTÜV WB 420-4 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |