General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.73 g/cm³ Show Material materials with Density of 2.73 g/cm³ | H12 | EN 573-3, EN 485 | ||
20.0 °C | 2.73 g/cm³ Show Material materials with Density of 2.73 g/cm³ | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | H12 | EN 573-3, EN 485 | |||
Bending angle 180° | 1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | H12 | EN 573-3, EN 485 | |||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H12 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H12 | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H12 | EN 573-3, EN 485 | ||||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H12 | EN 573-3, EN 485 | |||
69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | H12 | EN 573-3, EN 485 | ||||
20.0 °C | 65.0 GPa Show Material materials with Elastic modulus of 65.0 GPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongation | 3.0 % Show Material materials with Elongation of 3.0 % | H12 | EN 573-3, EN 485 | A50 | ||
4.0 % Show Material materials with Elongation of 4.0 % | H12 | EN 573-3, EN 485 | A50 | |||
5.0 % Show Material materials with Elongation of 5.0 % | H12 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H12 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Elongation of 7.0 % | H12 | EN 573-3, EN 485 | A50 | |||
8.0 % Show Material materials with Elongation of 8.0 % | H12 | EN 573-3, EN 485 | A100 | |||
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 38.0 [-] Show Material materials with Hardness, Brinell of 38.0 [-] | H12 | EN 573-3, EN 485 | |||
20.0 °C | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | H12 | EN 573-3, EN 485 | |||
20.0 °C | 26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Tensile strength | 120.0 - 160.0 MPa Show Material materials with Tensile strength of 120.0 - 160.0 MPa | H12 | EN 573-3, EN 485 | |||
20.0 °C | 125.0 - 165.0 MPa Show Material materials with Tensile strength of 125.0 - 165.0 MPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K | H12 | EN 573-3, EN 485 | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.15e-05 1/K | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K | H12 | EN 573-3, EN 485 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H12 | EN 573-3, EN 485 | ||
20 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
20 °C | 2.52e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H12 | EN 573-3, EN 485 | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.32e-05 1/K | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
200 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
200.0 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
300 °C | 2.52e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
300.0 °C | 2.52e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K | H12 | EN 573-3, EN 485, DIN 1725-1, EN 573-4 | Sheet, Strip | |
Melting point | 640.0 - 655.0 °C Show Material materials with Melting point of 640.0 - 655.0 °C | H12 | EN 573-3, EN 485 | ||
643.0 - 654.0 °C Show Material materials with Melting point of 643.0 - 654.0 °C | H12 | EN 573-3, EN 485 | |||
Specific heat capacity | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H12 | EN 573-3, EN 485 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
Thermal conductivity | 159.0 - 193.0 W/(m·K) Show Material materials with Thermal conductivity of 159.0 - 193.0 W/(m·K) | H12 | EN 573-3, EN 485 | ||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K) | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 24000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 24000000.0 - 29000000.0 S/m | H12 | EN 573-3, EN 485 | ||
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 29000000.0 S/m | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip | |
Electrical resistivity | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 4.17e-08 Ω·m | H12 | EN 573-3, EN 485 | ||
3.45e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 4.35e-08 Ω·m | H12 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 0.05 - 0.2 % Show Material materials with Copper of 0.05 - 0.2 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
0.70 % Show Material materials with Iron of 0.70 % | H12 | EN 573-3, EN 485 | ||
Manganese | 1.0 - 1.5 % Show Material materials with Manganese of 1.0 - 1.5 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip |
Silicon | 0.6 % Show Material materials with Silicon of 0.6 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 485 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |