General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H18 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 90° | 1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H18 | EN 573-3, EN 485 | |||
2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | H18 | EN 573-3, EN 485 | ||||
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H18 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 65.0 GPa Show Material materials with Elastic modulus of 65.0 GPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongation | 1.0 % Show Material materials with Elongation of 1.0 % | H18 | EN 573-3, EN 485 | A50 | ||
2.0 % Show Material materials with Elongation of 2.0 % | H18 | EN 573-3, EN 485 | A50 | |||
4.0 % Show Material materials with Elongation of 4.0 % | H18 | EN 573-3, EN 1592 | A100 | |||
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 69.0 [-] Show Material materials with Hardness, Brinell of 69.0 [-] | H18 | EN 573-3, EN 485 | |||
20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.5 Show Material materials with Shear modulus of 26.5 | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
Tensile strength | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | H18 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 215.0 - 235.0 MPa Show Material materials with Tensile strength of 215.0 - 235.0 MPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 215.0 - 255.0 MPa Show Material materials with Tensile strength of 215.0 - 255.0 MPa | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H18 | EN 573-3, EN 1592, EN 485 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H18 | EN 573-3, EN 1592, EN 485 | ||
Melting point | 630.0 - 654.0 °C Show Material materials with Melting point of 630.0 - 654.0 °C | H18 | EN 573-3, EN 1592, EN 485 | ||
Specific heat capacity | 20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal conductivity | 160.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K) | H18 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 200.0 W/(m·K) Show Material materials with Thermal conductivity of 200.0 W/(m·K) | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 23000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m | H18 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 28000000.0 S/m Show Material materials with Electrical conductivity of 28000000.0 S/m | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
Electrical resistivity | 4e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m | H18 | EN 573-3, EN 1592, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Copper | 0.3 % Show Material materials with Copper of 0.3 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | H18 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
0.70 % Show Material materials with Iron of 0.70 % | H18 | EN 573-3, EN 1592, EN 485 | ||
Magnesium | 0.2 - 0.6 % Show Material materials with Magnesium of 0.2 - 0.6 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Manganese | 1.0 - 1.5 % Show Material materials with Manganese of 1.0 - 1.5 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Silicon | 0.6 % Show Material materials with Silicon of 0.6 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H18 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / acceptable (H12) |