DIN 1725-1 Grade 3.0526 H14

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMn1Mg1 has similar properties like AlMn1, however it reaches higher strength (to F 26). It has also relatively high strength in the soft condition, but it is well cold fomrable. The alloy belongs to the nature-hard aluminum materials. A strength increase can be achieved, not by a purposeful heat treatment only by cold forming. It is very well warm and cold transformable and is suitable to the deep-drawing (no lappet formation). The alloy is very corrosion and sea water-steadily. The main field of application, the packing, determines the kind of semi-finished material standardized according to DIN 1788 and DIN 1745 (sheet metal and strip). Application: In the packing (DIN 59606) for cans (dose lower parts, abgestreckte doses), breaking covers and catches of all kinds. In the building industry for roofings (usually profile boards), claddings as well as for roll shutter and roll gates.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H14

EN 573-3, EN 1592, EN 485

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

2.5 °/t

Show Material materials with Bending angle 180° of 2.5 °/t

H14

EN 573-3, EN 485

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-3, EN 485

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H14

EN 573-3, EN 485

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H14

EN 573-3, EN 485

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H14

EN 573-3, EN 485

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3, EN 1592, EN 485

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3, EN 1592, EN 485

20.0 °C

65.0 - 71.0 GPa

Show Material materials with Elastic modulus of 65.0 - 71.0 GPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3, EN 485

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3, EN 485

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3, EN 485

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 1592

A100

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

A10

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Hardness, Brinell

67.0 [-]

Show Material materials with Hardness, Brinell of 67.0 [-]

H14

EN 573-3, EN 485

20.0 °C

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

20.0 °C

25.0 - 27.0 GPa

Show Material materials with Shear modulus of 25.0 - 27.0 GPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Tensile strength

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H14

EN 573-3, EN 1592

220.0 - 265.0 MPa

Show Material materials with Tensile strength of 220.0 - 265.0 MPa

H14

EN 573-3, EN 485

20.0 °C

220.0 - 260.0 MPa

Show Material materials with Tensile strength of 220.0 - 260.0 MPa

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1592, EN 485

-50.0 °C

2.15e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.15e-05 1/K

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

20 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

20 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

20 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

100.0 °C

2.32e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.32e-05 1/K

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

200 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

200.0 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

300 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

300.0 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

H14

EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4

Flat

Melting point

629.0 - 654.0 °C

Show Material materials with Melting point of 629.0 - 654.0 °C

H14

EN 573-3, EN 1592, EN 485

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

H14

EN 573-3, EN 1592, EN 485

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H14

EN 573-3, EN 1592, EN 485

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Thermal conductivity

160.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 180.0 W/(m·K)

H14

EN 573-3, EN 1592, EN 485

163 W/(m·K)

Show Material materials with Thermal conductivity of 163 W/(m·K)

H14

EN 573-3, EN 1592, EN 485

20.0 °C

160.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K)

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m

H14

EN 573-3, EN 1592, EN 485

24000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 S/m

H14

EN 573-3, EN 1592, EN 485

20.0 °C

20000000.0 - 24000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 24000000.0 S/m

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

Electrical resistivity

4e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m

H14

EN 573-3, EN 1592, EN 485

4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 4.17e-08 Ω·m

H14

EN 573-3, EN 1592, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.25 %

Show Material materials with Copper of 0.25 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H14

DIN 1725-1, EN 573-3, EN 573-4

Flat

0.70 %

Show Material materials with Iron of 0.70 %

H14

EN 573-3, EN 1592, EN 485

Magnesium

0.8 - 1.3 %

Show Material materials with Magnesium of 0.8 - 1.3 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H14

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12)