WL 3.3354 Grade 3.3354 H28

Want to keep this datasheet? Save it now in your required format

Description

The alloy is characterised by a good corrosion resistance. It is sea water steady and resistant to saline atmosphere. The Mg content increases the strength, but the cold forming capacity decreases. The material is nature hard, i.e. only by a cold forming and not by a purposeful heat treatment a strength increase can be attained. It is well polishable and anodisable. The splinter-giving machinability becomes better with increasing Mg content, just as the weldability. AlMg5 has the highest Mg content of the standardized AlMg alloys, so it is badly cold formable, but the strength is the highest, so that the employment is possible for statically more highly loaded constructions. The alloy is suitable for a splinter-giving machinig on automats. It possesses sensitivity to intergranular corrosion. By a purposeful heat treatment and/or by additive of Mn or Cr the inclination to the intergranular corrosion can be reduced. Application: In the optics, in the automobile engineering for body parts, in mechanical engineering (turned parts). For joining elements (solid rivets, blind rivets, riveting nuts and screws). In the building industry for carrying constructions as well as in shipbuilding considering the sensitivity to corrosion.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

2.64 g/cm³

Show Material materials with Density of 2.64 g/cm³

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

20.0 °C

67.0 - 72.0 GPa

Show Material materials with Elastic modulus of 67.0 - 72.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Hardness, Brinell

20.0 °C

90.0 [-]

Show Material materials with Hardness, Brinell of 90.0 [-]

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

20.0 °C

27.0 GPa

Show Material materials with Shear modulus of 27.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Shear strength

20.0 °C

180.0 MPa

Show Material materials with Shear strength of 180.0 MPa

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Tensile strength

20.0 °C

340.0 MPa

Show Material materials with Tensile strength of 340.0 MPa

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50.0 °C

2.25e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.25e-05 1/K

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

100.0 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

200.0 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

300.0 °C

2.61e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.61e-05 1/K

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

560.0 - 655.0 °C

Show Material materials with Melting point of 560.0 - 655.0 °C

Typical for Wrought 5000 Series Aluminium

Specific heat capacity

20.0 °C

904.0 J/(kg·K)

Show Material materials with Specific heat capacity of 904.0 J/(kg·K)

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Thermal conductivity

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Thermal conductivity of 110.0 - 140.0 W/(m·K)

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Electrical conductivity

20.0 °C

15000000.0 - 19000000.0 S/m

Show Material materials with Electrical conductivity of 15000000.0 - 19000000.0 S/m

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Electrical resistivity

3.3e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 - 5e-08 Ω·m

Typical for Wrought 5000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.2

Show Material materials with Chromium of 0.2

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Copper

0.1

Show Material materials with Copper of 0.1

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Iron

0.5

Show Material materials with Iron of 0.5

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Magnesium

4.5 - 5.6 %

Show Material materials with Magnesium of 4.5 - 5.6 %

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Manganese

0.1 - 0.6 %

Show Material materials with Manganese of 0.1 - 0.6 %

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Silicon

0.4

Show Material materials with Silicon of 0.4

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Titanium

0.2

Show Material materials with Titanium of 0.2

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Zinc

0.2

Show Material materials with Zinc of 0.2

H28

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354

Wire

Technological properties

Property
Workability

Good workability.