General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 70.0 Show Material materials with Elastic modulus of 70.0 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire | |
Elongation | 20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
Hardness, Brinell | 20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 72.0 [-] Show Material materials with Hardness, Brinell of 72.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.5 Show Material materials with Shear modulus of 26.5 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire | |
Shear strength | 20.0 °C | 130.0 MPa Show Material materials with Shear strength of 130.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
Tensile strength | 20.0 °C | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Tensile strength of 230.0 - 270.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.2e-05 - 2.5e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium | ||||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 560.0 - 655.0 °C Show Material materials with Melting point of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Specific heat capacity | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Specific heat capacity of 921.0 J/(kg·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire | |
Thermal conductivity | 20.0 °C | 167.0 Show Material materials with Thermal conductivity of 167.0 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 26000000.0 Show Material materials with Electrical conductivity of 26000000.0 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire | |
Electrical resistivity | 3.3e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.15 Show Material materials with Chromium of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Copper | 0.15 Show Material materials with Copper of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Iron | 0.5 Show Material materials with Iron of 0.5 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Magnesium | 1.7 - 2.4 % Show Material materials with Magnesium of 1.7 - 2.4 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Manganese | 0.1 - 0.5 % Show Material materials with Manganese of 0.1 - 0.5 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Silicon | 0.4 Show Material materials with Silicon of 0.4 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Titanium | 0.15 Show Material materials with Titanium of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Zinc | 0.15 Show Material materials with Zinc of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Flat, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |