General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
20.0 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elongation | 4.0 % Show Material materials with Elongation of 4.0 % | H12 | EN 573-3, EN 485 | A50 | ||
5.0 % Show Material materials with Elongation of 5.0 % | H12 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H12 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Elongation of 7.0 % | H12 | EN 573-3, EN 485 | A50 | |||
9.0 % Show Material materials with Elongation of 9.0 % | H12 | EN 573-3, EN 485 | A100 | |||
9.0 % Show Material materials with Elongation of 9.0 % | H12 | EN 573-3, EN 485, EN 754 | A50 | |||
10.0 % Show Material materials with Elongation of 10.0 % | H12 | EN 573-3, EN 1592, EN 754 | A100 | |||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | H12 | EN 573-3, EN 754 | |||
66.0 [-] Show Material materials with Hardness, Brinell of 66.0 [-] | H12 | EN 573-3, EN 485 | ||||
20.0 °C | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.5 Show Material materials with Shear modulus of 26.5 | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | |
Tensile strength | 210.0 - 270.0 MPa Show Material materials with Tensile strength of 210.0 - 270.0 MPa | H12 | EN 573-3, EN 754 | |||
220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | H12 | EN 573-3, EN 1592 | ||||
220.0 - 270.0 MPa Show Material materials with Tensile strength of 220.0 - 270.0 MPa | H12 | EN 573-3, EN 485 | ||||
20.0 °C | 220.0 - 260.0 MPa Show Material materials with Tensile strength of 220.0 - 260.0 MPa | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | Long | |
150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Melting point | 620.0 - 650.0 °C Show Material materials with Melting point of 620.0 - 650.0 °C | H12 | EN 573-3, EN 1592, EN 485, EN 754 | |||
Specific heat capacity | 879.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Thermal conductivity | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K) | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Electrical resistivity | 4e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m | H12 | EN 573-3, EN 1592, EN 485, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.3 % Show Material materials with Chromium of 0.3 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | H12 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
0.50 % Show Material materials with Iron of 0.50 % | H12 | EN 573-3, EN 1592, EN 485, EN 754 | ||
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Manganese | 0.5 - 1.1 % Show Material materials with Manganese of 0.5 - 1.1 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H12 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485, EN 754 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |