DIN 1725-1 Grade 3.3527 H28

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMg2Mn0,8 has similar characteristics as the alloy AlMg1,8. The additive of Mn (>0,6%) causes an increase of the heat resistance (up to 150°C) of the material and the recrystallisation limit. The result of the last is, that in case of extruded profiles the strength in longitudinal direction increases. The material is characterised by a good corrosion resistance. It is sea water steady and steady against saline atmosphere. With the Mg content the strength increases, the cold forming capacity decreases. The alloy is nature hard, i.e. that only by a cold forming shaping however by a purposeful heat treatment a strength increase cannot be attained. The splinter-giving workability and the weldability are improved with increasing Mg content. Application: In the apparatus engineering for receivers accordint to AD-W6/1 and according to VdTUEV-Werkstoffblaetter, for compressed gas tanks (pipings), for very low-temperature tanks and for temperatures to 250 °C. In the automobile engineering for utilizable superstructures, silo trucks, in shipbuilding for trunk and superstructures. In the building industry for roofings, claddings, for carrying constructions according to DIN 4173 and sun protection facilities as well as for furniture (including camping furniture).

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H28

EN 573-3, EN 1592, EN 485

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H28

EN 573-3, EN 1592, EN 485

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Elongation

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3, EN 1592

A100

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3, EN 485

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H28

EN 573-3, EN 485

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Hardness, Brinell

87.0 [-]

Show Material materials with Hardness, Brinell of 87.0 [-]

H28

EN 573-3, EN 485

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

20.0 °C

26.5

Show Material materials with Shear modulus of 26.5

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Tensile strength

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H28

EN 573-3, EN 1592

290.0 MPa

Show Material materials with Tensile strength of 290.0 MPa

H28

EN 573-3, EN 485

20.0 °C

260.0 - 300.0 MPa

Show Material materials with Tensile strength of 260.0 - 300.0 MPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H28

EN 573-3, EN 1592, EN 485

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H28

EN 573-3, EN 1592, EN 485

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

620.0 - 650.0 °C

Show Material materials with Melting point of 620.0 - 650.0 °C

H28

EN 573-3, EN 1592, EN 485

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

20.0 °C

140.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K)

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Electrical resistivity

4e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m

H28

EN 573-3, EN 1592, EN 485

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

0.50 %

Show Material materials with Iron of 0.50 %

H28

EN 573-3, EN 1592, EN 485

Magnesium

1.6 - 2.5 %

Show Material materials with Magnesium of 1.6 - 2.5 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Manganese

0.5 - 1.1 %

Show Material materials with Manganese of 0.5 - 1.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485

Flat

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)