General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | H22 | EN 573-3, EN 485 | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 120.0 MPa Show Material materials with Bending Fatigue Strength of 120.0 MPa | H22 | EN 573-3, EN 485 | |||
Bending angle 180° | 1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | H22 | EN 573-3, EN 485 | |||
2.0 °/t Show Material materials with Bending angle 180° of 2.0 °/t | H22 | EN 573-3, EN 485 | ||||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H22 | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H22 | EN 573-3, EN 485 | ||||
2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | H22 | EN 573-3, EN 485 | ||||
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | H22 | EN 573-3, EN 485 | ||||
Elastic modulus | 70.5 GPa Show Material materials with Elastic modulus of 70.5 GPa | H22 | EN 573-3, EN 485 | |||
20.0 °C | 72.0 GPa Show Material materials with Elastic modulus of 72.0 GPa | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
Elongation | 5.0 % Show Material materials with Elongation of 5.0 % | H22 | EN 573-3, EN 485 | A50 | ||
6.0 % Show Material materials with Elongation of 6.0 % | H22 | EN 573-3, EN 485 | A50 | |||
7.0 % Show Material materials with Elongation of 7.0 % | H22 | EN 573-3, EN 485 | A50 | |||
8.0 % Show Material materials with Elongation of 8.0 % | H22 | EN 573-3, EN 485 | A50 | |||
9.0 % Show Material materials with Elongation of 9.0 % | H22 | EN 573-3, EN 485 | A100 | |||
10.0 % Show Material materials with Elongation of 10.0 % | H22 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
Hardness, Brinell | 74.0 [-] Show Material materials with Hardness, Brinell of 74.0 [-] | H22 | EN 573-3, EN 485 | |||
20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | H22 | EN 573-3, EN 485 | |||
20.0 °C | 27.0 GPa Show Material materials with Shear modulus of 27.0 GPa | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
Tensile strength | 250.0 - 305.0 MPa Show Material materials with Tensile strength of 250.0 - 305.0 MPa | H22 | EN 573-3, EN 485 | |||
20.0 °C | 245.0 - 305.0 MPa Show Material materials with Tensile strength of 245.0 - 305.0 MPa | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.1899999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1899999999999997e-05 1/K | H22 | EN 573-3, EN 485 | ||
-50.0 °C | 2.19e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.19e-05 1/K | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
20 °C | 2.1899999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1899999999999997e-05 1/K | H22 | EN 573-3, EN 485 | |||
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | H22 | EN 573-3, EN 485 | |||
20 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
20 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
100 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | H22 | EN 573-3, EN 485 | |||
100.0 °C | 2.37e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.37e-05 1/K | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
200 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
200.0 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
300 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
300.0 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | H22 | EN 573-3, EN 485, DIN 1725-1, EN 573-4, VdTÜV WB 386 | Sheet | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 602.0 - 646.0 °C Show Material materials with Melting point of 602.0 - 646.0 °C | H22 | EN 573-3, EN 485 | |||
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H22 | EN 573-3, EN 485 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | ||
Thermal conductivity | 130.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K) | H22 | EN 573-3, EN 485 | |||
20.0 °C | 150.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 W/(m·K) | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 19000000.0 - 21000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m | H22 | EN 573-3, EN 485 | ||
20.0 °C | 21000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 S/m | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet | |
Electrical resistivity | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m | H22 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.05 - 0.2 % Show Material materials with Chromium of 0.05 - 0.2 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Iron | 0.4 % Show Material materials with Iron of 0.4 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386 | Sheet |
0.40 % Show Material materials with Iron of 0.40 % | H22 | EN 573-3, EN 485 | ||
Magnesium | 2.4 - 3.0 % Show Material materials with Magnesium of 2.4 - 3.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Manganese | 0.5 - 1.0 % Show Material materials with Manganese of 0.5 - 1.0 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Titanium | 0.2 % Show Material materials with Titanium of 0.2 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H22 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 386, EN 485 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |