General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
2.78 g/cm³ Show Material materials with Density of 2.78 g/cm³ | T4 | EN 573-3, EN 1301, EN 485, EN 586 | |||
20.0 °C | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 140.0 MPa Show Material materials with Bending Fatigue Strength of 140.0 MPa | T4 | EN 573-3, EN 485, EN 586 | |||
Bending angle 180° | 4.0 °/t Show Material materials with Bending angle 180° of 4.0 °/t | T4 | EN 573-3, EN 485 | |||
5.0 °/t Show Material materials with Bending angle 180° of 5.0 °/t | T4 | EN 573-3, EN 485 | ||||
Elastic modulus | 73.0 GPa Show Material materials with Elastic modulus of 73.0 GPa | T4 | EN 573-3, EN 1301, EN 485, EN 586 | |||
20.0 °C | 70.0 - 74.5 GPa Show Material materials with Elastic modulus of 70.0 - 74.5 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire | ||
Elongation | 8.0 % Show Material materials with Elongation of 8.0 % | T4 | EN 573-3, EN 586 | A100 | ||
12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3, EN 485 | A50 | |||
14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3, EN 485 | A50 | |||
18.0 % Show Material materials with Elongation of 18.0 % | T4 | EN 573-3, EN 1301 | ||||
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
Hardness, Brinell | 100.0 [-] Show Material materials with Hardness, Brinell of 100.0 [-] | T4 | EN 573-3, EN 586 | |||
120.0 [-] Show Material materials with Hardness, Brinell of 120.0 [-] | T4 | EN 573-3, EN 485 | ||||
20.0 °C | 105.0 [-] Show Material materials with Hardness, Brinell of 105.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging | ||
20.0 °C | 110.0 [-] Show Material materials with Hardness, Brinell of 110.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 27.4 GPa Show Material materials with Shear modulus of 27.4 GPa | T4 | EN 573-3, EN 1301, EN 485, EN 586 | |||
20.0 °C | 27.0 - 28.0 GPa Show Material materials with Shear modulus of 27.0 - 28.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire | ||
Tensile strength | 420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T4 | EN 573-3, EN 1301, EN 586 | |||
425.0 MPa Show Material materials with Tensile strength of 425.0 MPa | T4 | EN 573-3, EN 485 | ||||
20.0 °C | 420.0 MPa Show Material materials with Tensile strength of 420.0 MPa | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.11e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | |
20 °C | 2.11e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.11e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2899999999999998e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
200 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
300 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
Melting point | 505.0 - 640.0 °C Show Material materials with Melting point of 505.0 - 640.0 °C | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
505.0 - 635.0 °C Show Material materials with Melting point of 505.0 - 635.0 °C | T4 | EN 573-3, EN 1301, EN 485, EN 586 | |||
Specific heat capacity | 875.0 J/(kg·K) Show Material materials with Specific heat capacity of 875.0 J/(kg·K) | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20.0 °C | 875.0 J/(kg·K) Show Material materials with Specific heat capacity of 875.0 J/(kg·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire | |
Thermal conductivity | 121.0 - 193.0 W/(m·K) Show Material materials with Thermal conductivity of 121.0 - 193.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 17000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 29000000.0 S/m | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 - 21000000.0 S/m | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire | |
Electrical resistivity | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 5.88e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
4.76e-08 - 5.56e-08 Ω·m Show Material materials with Electrical resistivity of 4.76e-08 - 5.56e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 485, EN 586 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Copper | 3.8 - 4.9 % Show Material materials with Copper of 3.8 - 4.9 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | T4 | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Wire |
0.50 % Show Material materials with Iron of 0.50 % | T4 | EN 573-3, EN 1301, EN 485, EN 586 | ||
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Manganese | 0.3 - 0.9 % Show Material materials with Manganese of 0.3 - 0.9 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Silicon | 0.5 % Show Material materials with Silicon of 0.5 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 586 | Forging, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O) |