General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 68.0 - 73.0 GPa Show Material materials with Elastic modulus of 68.0 - 73.0 GPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire | |
Elongation | 20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A100 |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Rod | ||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A10 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Strip, Tube | A10 | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Rod, Sheet | ||
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Tube | A10 | |
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Strip, Tube | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Flat | A10 | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Tube | ||
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Flat | ||
Hardness, Brinell | 20.0 °C | 80.0 [-] Show Material materials with Hardness, Brinell of 80.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Tube | |
20.0 °C | 85.0 [-] Show Material materials with Hardness, Brinell of 85.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Flat | ||
20.0 °C | 90.0 - 95.0 [-] Show Material materials with Hardness, Brinell of 90.0 - 95.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet | ||
20.0 °C | 90.0 [-] Show Material materials with Hardness, Brinell of 90.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet | ||
20.0 °C | 95.0 [-] Show Material materials with Hardness, Brinell of 95.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Strip, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.0 - 27.0 GPa Show Material materials with Shear modulus of 26.0 - 27.0 GPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire | |
Tensile strength | 20.0 °C | 270.0 MPa Show Material materials with Tensile strength of 270.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Rod | |
20.0 °C | 275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Tube | ||
20.0 °C | 295.0 MPa Show Material materials with Tensile strength of 295.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet | ||
20.0 °C | 300.0 MPa Show Material materials with Tensile strength of 300.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Rod | ||
20.0 °C | 310.0 MPa Show Material materials with Tensile strength of 310.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Tube | ||
20.0 °C | 315.0 MPa Show Material materials with Tensile strength of 315.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Sheet, Strip | ||
20.0 °C | 320.0 MPa Show Material materials with Tensile strength of 320.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium | ||||
Melting point | 555.0 - 655.0 °C Show Material materials with Melting point of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium | ||||
Specific heat capacity | 887.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Thermal conductivity | 20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K) | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire | |
Electrical resistivity | 2.9e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.25 Show Material materials with Chromium of 0.25 | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Copper | 0.1 Show Material materials with Copper of 0.1 | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Iron | 0.5 Show Material materials with Iron of 0.5 | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Manganese | 0.4 - 1.0 % Show Material materials with Manganese of 0.4 - 1.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Silicon | 0.7 - 1.3 % Show Material materials with Silicon of 0.7 - 1.3 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Titanium | 0.1 Show Material materials with Titanium of 0.1 | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Zinc | 0.2 Show Material materials with Zinc of 0.2 | T8 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Profile, Rod, Sheet, Flat, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |