General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Elongation | 20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | A10 |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | A10 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | ||
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | ||
Hardness, Brinell | 20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | |
20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.0 - 26.5 GPa Show Material materials with Shear modulus of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Tensile strength | 20.0 °C | 210.0 MPa Show Material materials with Tensile strength of 210.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile | |
20.0 °C | 240.0 MPa Show Material materials with Tensile strength of 240.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Thermal
Property | Value | Comment |
---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Melting point | 555.0 - 655.0 °C Show Material materials with Melting point of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Specific heat capacity | 887.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Thermal conductivity | 170.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Electrical
Property | Value | Comment |
---|---|---|
Electrical conductivity | 21000000.0 - 34000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
Electrical resistivity | 2.9e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 0.05 - 0.2 % Show Material materials with Copper of 0.05 - 0.2 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Iron | 0.04 Show Material materials with Iron of 0.04 | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Magnesium | 0.35 - 0.7 % Show Material materials with Magnesium of 0.35 - 0.7 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Manganese | 0.03 Show Material materials with Manganese of 0.03 | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Silicon | 0.35 - 0.7 % Show Material materials with Silicon of 0.35 - 0.7 % | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Titanium | 0.01 Show Material materials with Titanium of 0.01 | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Zinc | 0.04 Show Material materials with Zinc of 0.04 | T8 | DIN 1725-1, EN 573-3, EN 573-4 | Profile |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |