EN 573-3 Grade 3.3211 O

View suppliers (3)
Want to keep this datasheet? Save it now in your required format

Description

DIN 3.3211 is a readily available alloy that has good surface finish and ability to be anodized.Easy of weldability and brazability with nice surface finish. Resistance to corrosion from seawater and atmospheric conditions. Suitable for hot forging.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

60.0 MPa

Show Material materials with Bending Fatigue Strength of 60.0 MPa

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

O

EN 573-3, EN 485

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

O

EN 573-3, EN 1386, EN 485

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

68.3 - 69.6 GPa

Show Material materials with Elastic modulus of 68.3 - 69.6 GPa

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Elongation

6.0 %

Show Material materials with Elongation of 6.0 %

O

EN 573-3, EN 1386

A50

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3, EN 1386

A50

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3, EN 1386

A50

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3, EN 1386

A50

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3, EN 1386

A100

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 485, EN 754, EN 755

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 485

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 485, EN 754, EN 755

A100

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3, EN 485

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet

A10

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

WL 3.3214-1, DIN 1725-1

Sheet

A50 Transverse

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Strip, Sheet

A10

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

WL 3.3214-1, DIN 1725-1

Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

WL 3.3214-1, DIN 1725-1

Sheet

A50 Transverse

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Strip, Sheet

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

WL 3.3214-1, DIN 1725-1

Sheet

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

WL 3.3214-1, DIN 1725-1

Sheet

Transverse

Hardness, Brinell

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

O

EN 573-3, EN 485

20.0 °C

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Strip, Sheet, Tube

20.0 °C

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

O

WL 3.3214-1, DIN 1725-1

Sheet

Transverse

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.3 GPa

Show Material materials with Shear modulus of 26.3 GPa

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

26.2 GPa

Show Material materials with Shear modulus of 26.2 GPa

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Tensile strength

150.0

Show Material materials with Tensile strength of 150.0

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

150.0

Show Material materials with Tensile strength of 150.0

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Strip, Sheet, Tube

20.0 °C

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

O

WL 3.3214-1, DIN 1725-1

Sheet

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Melting point

580.0 - 640.0 °C

Show Material materials with Melting point of 580.0 - 640.0 °C

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

580.0 - 650.0 °C

Show Material materials with Melting point of 580.0 - 650.0 °C

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Specific heat capacity

20.0 °C

870.0 J/(kg·K)

Show Material materials with Specific heat capacity of 870.0 J/(kg·K)

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Thermal conductivity

155.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 155.0 - 180.0 W/(m·K)

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

170.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 170.0 - 200.0 W/(m·K)

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

150.0 - 165.0 W/(m·K)

Show Material materials with Thermal conductivity of 150.0 - 165.0 W/(m·K)

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

22000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 30000000.0 S/m

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

23000000.0 - 27000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 27000000.0 S/m

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

20.0 °C

20000000.0 - 30000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 30000000.0 S/m

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip

Electrical resistivity

3.33e-08 - 4.55e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 - 4.55e-08 Ω·m

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

3.7e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.7e-08 - 4.35e-08 Ω·m

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.04 - 0.35 %

Show Material materials with Chromium of 0.04 - 0.35 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Copper

0.15 - 0.4 %

Show Material materials with Copper of 0.15 - 0.4 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Iron

0.7 %

Show Material materials with Iron of 0.7 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1

Sheet, Strip, Tube

0.70 %

Show Material materials with Iron of 0.70 %

O

EN 573-3, EN 1386, EN 485, EN 754, EN 755

Magnesium

0.8 - 1.2 %

Show Material materials with Magnesium of 0.8 - 1.2 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Manganese

0.15 %

Show Material materials with Manganese of 0.15 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Silicon

0.4 - 0.8 %

Show Material materials with Silicon of 0.4 - 0.8 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

O

DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755

Sheet, Strip, Tube

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable

Corrosion properties

Seawater: good to acceptable, weathering: good

Workability

Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O)