General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 68.3 - 69.6 GPa Show Material materials with Elastic modulus of 68.3 - 69.6 GPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat | |
Elongation | 20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet | |
20.0 °C | 8.0 % Show Material materials with Elongation of 8.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Flat | A10 | |
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Flat | ||
Hardness, Brinell | 20.0 °C | 90.0 [-] Show Material materials with Hardness, Brinell of 90.0 [-] | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Flat, Sheet | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 26.2 Show Material materials with Shear modulus of 26.2 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat | |
Tensile strength | 20.0 °C | 290.0 MPa Show Material materials with Tensile strength of 290.0 MPa | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Flat, Sheet |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 1.6e-05 - 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium | ||||
Melting point | 555.0 - 655.0 °C Show Material materials with Melting point of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium | ||||
Specific heat capacity | 20.0 °C | 870.0 J/(kg·K) Show Material materials with Specific heat capacity of 870.0 J/(kg·K) | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat | |
Thermal conductivity | 20.0 °C | 150.0 - 165.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 - 165.0 W/(m·K) | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 20000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 30000000.0 S/m | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat | |
Electrical resistivity | 2.9e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.04 - 0.35 % Show Material materials with Chromium of 0.04 - 0.35 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Iron | 0.7 Show Material materials with Iron of 0.7 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Manganese | 0.15 Show Material materials with Manganese of 0.15 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Titanium | 0.15 Show Material materials with Titanium of 0.15 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Zinc | 0.25 Show Material materials with Zinc of 0.25 | T8 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |