DIN 1712-3 Grade 3.0257 H14

Want to keep this datasheet? Save it now in your required format

Description

Pure aluminium Electrical conductivity alloy according to DIN, ensured by the German electrotechnical commission for electro-technology with, also in accordance to DIN 40 501 part of 1 to part of 4. This material has a very good electrical and good thermal conductivity, however only relatively low mechanical strength. Forming capacity and chemical as well as weather proofness are very good. Application: Roll bond, z-bond, wiring loom-change with particularly high requirements.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H14

EN 573-3, EN 755

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire, Rod, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3, EN 755

Elongation

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 755

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 755

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire

A200

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Tube

A10

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Rod

A10

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Tube

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Rod

Hardness, Brinell

33.0 [-]

Show Material materials with Hardness, Brinell of 33.0 [-]

H14

EN 573-3, EN 755

20.0 °C

28.0 - 38.0 [-]

Show Material materials with Hardness, Brinell of 28.0 - 38.0 [-]

H14

DIN 1712-3, EN 573-3, EN 573-4

Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire, Rod, Tube

Tensile strength

100.0 - 135.0 MPa

Show Material materials with Tensile strength of 100.0 - 135.0 MPa

H14

EN 573-3, EN 755

20.0 °C

90.0 - 130.0 MPa

Show Material materials with Tensile strength of 90.0 - 130.0 MPa

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

100.0 - 140.0 MPa

Show Material materials with Tensile strength of 100.0 - 140.0 MPa

H14

DIN 1712-3, EN 573-3, EN 573-4, EN 755

Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 755

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 755

Melting point

658.0 °C

Show Material materials with Melting point of 658.0 °C

H14

EN 573-3, EN 755

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire, Rod, Tube

Thermal conductivity

230 W/(m·K)

Show Material materials with Thermal conductivity of 230 W/(m·K)

H14

EN 573-3, EN 755

20.0 °C

230.0 W/(m·K)

Show Material materials with Thermal conductivity of 230.0 W/(m·K)

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire, Rod, Tube

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

34500000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35500000.0 S/m

H14

EN 573-3, EN 755

Electrical resistivity

2.82e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.82e-08 - 2.9e-08 Ω·m

H14

EN 573-3, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

H14

EN 573-3, EN 755

Copper

0.02 %

Show Material materials with Copper of 0.02 %

H14

DIN 1712-3, EN 573-3, EN 573-4, EN 755

Wire, Rod, Tube

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H14

DIN 1712-3, EN 573-3, EN 573-4

Wire, Rod, Tube

0.40 %

Show Material materials with Iron of 0.40 %

H14

EN 573-3, EN 755

Magnesium

0.05 %

Show Material materials with Magnesium of 0.05 %

H14

DIN 1712-3, EN 573-3, EN 573-4, EN 755

Wire, Rod, Tube

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

H14

DIN 1712-3, EN 573-3, EN 573-4, EN 755

Wire, Rod, Tube

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H14

DIN 1712-3, EN 573-3, EN 573-4, EN 755

Wire, Rod, Tube

Technological properties

Property
Brazing

Excellent

Workability

Excellent workability.