General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H12 | EN 573-3, EN 755 | |||
Elongation | 15.0 % Show Material materials with Elongation of 15.0 % | H12 | EN 573-3, EN 755 | A50 | ||
15.0 % Show Material materials with Elongation of 15.0 % | H12 | EN 573-3, EN 755 | A100 | |||
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Hardness, Brinell | 25.0 [-] Show Material materials with Hardness, Brinell of 25.0 [-] | H12 | EN 573-3, EN 755 | |||
20.0 °C | 25.0 - 35.0 [-] Show Material materials with Hardness, Brinell of 25.0 - 35.0 [-] | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 25.0 - 26.5 GPa Show Material materials with Shear modulus of 25.0 - 26.5 GPa | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
Tensile strength | 80.0 MPa Show Material materials with Tensile strength of 80.0 MPa | H12 | EN 573-3, EN 755 | |||
20.0 °C | 90.0 - 130.0 MPa Show Material materials with Tensile strength of 90.0 - 130.0 MPa | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H12 | EN 573-3, EN 755 | |
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H12 | EN 573-3, EN 755 | ||
Melting point | 658.0 °C Show Material materials with Melting point of 658.0 °C | H12 | EN 573-3, EN 755 | ||
Specific heat capacity | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Specific heat capacity of 921.0 J/(kg·K) | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal conductivity | 230 W/(m·K) Show Material materials with Thermal conductivity of 230 W/(m·K) | H12 | EN 573-3, EN 755 | ||
20.0 °C | 230.0 W/(m·K) Show Material materials with Thermal conductivity of 230.0 W/(m·K) | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 34500000.0 - 35500000.0 S/m Show Material materials with Electrical conductivity of 34500000.0 - 35500000.0 S/m | H12 | EN 573-3, EN 755 |
Electrical resistivity | 2.82e-08 - 2.9e-08 Ω·m Show Material materials with Electrical resistivity of 2.82e-08 - 2.9e-08 Ω·m | H12 | EN 573-3, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H12 | EN 573-3, EN 755 | |
Copper | 0.02 % Show Material materials with Copper of 0.02 % | H12 | DIN 1712-3, EN 573-3, EN 573-4, EN 755 | Sheet, Strip |
Iron | 0.4 % Show Material materials with Iron of 0.4 % | H12 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip |
0.40 % Show Material materials with Iron of 0.40 % | H12 | EN 573-3, EN 755 | ||
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | H12 | DIN 1712-3, EN 573-3, EN 573-4, EN 755 | Sheet, Strip |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | H12 | DIN 1712-3, EN 573-3, EN 573-4, EN 755 | Sheet, Strip |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H12 | DIN 1712-3, EN 573-3, EN 573-4, EN 755 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |