EN 573-3 Grade AW-3103 H18

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.06 mm

Show Material materials with Thickness of 0.06 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.06 mm

Coil, Sheet

4.0 mm

Show Material materials with Thickness of 4.0 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

4.0 mm

Coil, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

75.0 MPa

Show Material materials with Bending Fatigue Strength of 75.0 MPa

H18

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

3.0 °/t

Show Material materials with Bending angle 90° of 3.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

69.0 - 69.5 GPa

Show Material materials with Elastic modulus of 69.0 - 69.5 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

69.5 - 70.0 GPa

Show Material materials with Elastic modulus of 69.5 - 70.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3

Coil, Sheet, Foil, Rod, Flat, Seamless Tube, Tube, Wire

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Elongation

-196.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

H18

EN 573-3

-80.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H18

EN 573-3

-20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H18

EN 573-3

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

1.0 - 2.0 %

Show Material materials with Elongation of 1.0 - 2.0 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Foil

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Foil, Flat

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Seamless Tube

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3

Rod, Tube

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3

Wire

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H18

EN 573-3

100.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H18

EN 573-3

150.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

H18

EN 573-3

200.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H18

EN 573-3

260.0 °C

60.0 %

Show Material materials with Elongation of 60.0 %

H18

EN 573-3

320.0 °C

70.0 %

Show Material materials with Elongation of 70.0 %

H18

EN 573-3

370.0 °C

70.0 %

Show Material materials with Elongation of 70.0 %

H18

EN 573-3

Hardness, Brinell

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

55.0 [-]

Show Material materials with Hardness, Brinell of 55.0 [-]

H18

EN 573-3

Rod, Tube

20.0 °C

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H18

EN 573-3

Flat

Hardness, HBW

62 [-]

Show Material materials with Hardness, HBW of 62 [-]

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Shear modulus of 24.0 - 26.5 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

24.0 - 26.1 GPa

Show Material materials with Shear modulus of 24.0 - 26.1 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

26.1 - 26.5 GPa

Show Material materials with Shear modulus of 26.1 - 26.5 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Tensile strength

-196.0 °C

298.0 MPa

Show Material materials with Tensile strength of 298.0 MPa

H18

EN 573-3

-80.0 °C

225.0 MPa

Show Material materials with Tensile strength of 225.0 MPa

H18

EN 573-3

-20.0 °C

214.0 MPa

Show Material materials with Tensile strength of 214.0 MPa

H18

EN 573-3

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H18

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H18

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H18

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

185 MPa

Show Material materials with Tensile strength of 185 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H18

EN 573-3

Wire

20.0 °C

175.0 MPa

Show Material materials with Tensile strength of 175.0 MPa

H18

EN 573-3

Foil

20.0 °C

175.0 - 230.0 MPa

Show Material materials with Tensile strength of 175.0 - 230.0 MPa

H18

EN 573-3

Foil

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H18

EN 573-3

Rod, Tube

20.0 °C

185.0 - 230.0 MPa

Show Material materials with Tensile strength of 185.0 - 230.0 MPa

H18

EN 573-3, EN 546

Foil, Strip, Sheet, Plate, Bar, Rod, Tube

20.0 °C

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H18

EN 573-3

Foil, Flat

20.0 °C

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H18

EN 573-3

Flat

Transverse

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H18

EN 573-3

Seamless Tube

20.0 °C

204.0 MPa

Show Material materials with Tensile strength of 204.0 MPa

H18

EN 573-3

100.0 °C

183.0 MPa

Show Material materials with Tensile strength of 183.0 MPa

H18

EN 573-3

150.0 °C

163.0 MPa

Show Material materials with Tensile strength of 163.0 MPa

H18

EN 573-3

200.0 °C

98.0 MPa

Show Material materials with Tensile strength of 98.0 MPa

H18

EN 573-3

260.0 °C

53.0 MPa

Show Material materials with Tensile strength of 53.0 MPa

H18

EN 573-3

320.0 °C

28.0 MPa

Show Material materials with Tensile strength of 28.0 MPa

H18

EN 573-3

370.0 °C

21.0 MPa

Show Material materials with Tensile strength of 21.0 MPa

H18

EN 573-3

Yield strength

-196.0 °C

232.0 MPa

Show Material materials with Yield strength of 232.0 MPa

H18

EN 573-3

RP02

-80.0 °C

204.0 MPa

Show Material materials with Yield strength of 204.0 MPa

H18

EN 573-3

RP02

-20.0 °C

197.0 MPa

Show Material materials with Yield strength of 197.0 MPa

H18

EN 573-3

RP02

145.0 MPa

Show Material materials with Yield strength of 145.0 MPa

H18

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H18

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

165.0 MPa

Show Material materials with Yield strength of 165.0 MPa

H18

EN 573-3, EN 1301, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

165 MPa

Show Material materials with Yield strength of 165 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

20.0 °C

145.0 MPa

Show Material materials with Yield strength of 145.0 MPa

H18

EN 573-3

Rod, Tube

RP02

20.0 °C

160.0 MPa

Show Material materials with Yield strength of 160.0 MPa

H18

EN 573-3

Foil

RP02

20.0 °C

165.0 MPa

Show Material materials with Yield strength of 165.0 MPa

H18

EN 573-3

Wire, Flat

RP02

20.0 °C

165.0 MPa

Show Material materials with Yield strength of 165.0 MPa

H18

EN 573-3

Flat

RP02 Transverse

20.0 °C

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H18

EN 573-3

Seamless Tube

RP02

20.0 °C

190.0 MPa

Show Material materials with Yield strength of 190.0 MPa

H18

EN 573-3

RP02

100.0 °C

148.0 MPa

Show Material materials with Yield strength of 148.0 MPa

H18

EN 573-3

RP02

150.0 °C

113.0 MPa

Show Material materials with Yield strength of 113.0 MPa

H18

EN 573-3

RP02

200.0 °C

63.0 MPa

Show Material materials with Yield strength of 63.0 MPa

H18

EN 573-3

RP02

260.0 °C

28.0 MPa

Show Material materials with Yield strength of 28.0 MPa

H18

EN 573-3

RP02

320.0 °C

17.0 MPa

Show Material materials with Yield strength of 17.0 MPa

H18

EN 573-3

RP02

370.0 °C

13.0 MPa

Show Material materials with Yield strength of 13.0 MPa

H18

EN 573-3

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

0.000025 1/K

Show Material materials with Coefficient of thermal expansion of 0.000025 1/K

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20-100°C

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

892.0 - 893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 - 893.0 J/(kg·K)

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

892.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 J/(kg·K)

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Thermal conductivity

176 W/(m·K)

Show Material materials with Thermal conductivity of 176 W/(m·K)

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K)

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube, Wire

20.0 °C

160.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 W/(m·K)

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

22000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube, Wire

20.0 °C

22000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 29000000.0 S/m

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Electrical resistivity

3.57e-08 - 4.55e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 4.55e-08 Ω·m

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 Ω·m

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

3.4e-08 - 4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.1e-08 Ω·m

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

3.4e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.5e-08 Ω·m

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 Ω·m

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

20.0 °C

4.1e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 - 4.5e-08 Ω·m

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar

0.1 %

Show Material materials with Chromium of 0.1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar

0.1 %

Show Material materials with Copper of 0.1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H18

EN 573-3

Foil, Rod, Flat, Seamless Tube, Tube, Wire

0.70 %

Show Material materials with Iron of 0.70 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

0.7 %

Show Material materials with Iron of 0.7 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Magnesium

0.3 %

Show Material materials with Magnesium of 0.3 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar

0.3 %

Show Material materials with Magnesium of 0.3 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Manganese

0.9 - 1.5 %

Show Material materials with Manganese of 0.9 - 1.5 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar, Coil, Sheet

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar

0.5 %

Show Material materials with Silicon of 0.5 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H18

EN 573-3, EN 1301, EN 1592, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Seamless Tube, Tube, Wire, Strip, Sheet, Plate, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers

Brazing

hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12)