EN 573-3 Grade AW-5005 H19

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5005 is a lean aluminum magnesium alloy with low density and excellent thermal conductivity. This medium strength non-heat-treatable alloy is known for its corrosion resistance in alkaline marine situations. Aluminum EN AW-5005 is readily machinable, and can be welded using TIG and MIG methods. It is important to note that anodizing is a critical part to how Aluminum EN AW-5005 is used.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H19

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Flat, Coil, Sheet, Strip

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.1 mm

Show Material materials with Thickness of 0.1 mm

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

0.1 mm

Coil, Sheet, Strip

4.0 mm

Show Material materials with Thickness of 4.0 mm

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

4.0 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Bending angle 90°

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H19

EN 573-3

Flat

Hardness, Brinell

64.0 [-]

Show Material materials with Hardness, Brinell of 64.0 [-]

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

64.0 [-]

Show Material materials with Hardness, Brinell of 64.0 [-]

H19

EN 573-3

Flat

Hardness, HBW

64 [-]

Show Material materials with Hardness, HBW of 64 [-]

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H19

EN 573-3

Flat

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H19

EN 573-3

Flat

Tensile strength

205.0 MPa

Show Material materials with Tensile strength of 205.0 MPa

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

205 MPa

Show Material materials with Tensile strength of 205 MPa

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20.0 °C

205.0 MPa

Show Material materials with Tensile strength of 205.0 MPa

H19

EN 573-3

Flat

Transverse

20.0 °C

205.0 MPa

Show Material materials with Tensile strength of 205.0 MPa

H19

EN 573-3

Flat

Yield strength

185.0 MPa

Show Material materials with Yield strength of 185.0 MPa

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

RP02

185 MPa

Show Material materials with Yield strength of 185 MPa

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20.0 °C

185.0 MPa

Show Material materials with Yield strength of 185.0 MPa

H19

EN 573-3

Flat

RP02 Transverse

20.0 °C

185.0 MPa

Show Material materials with Yield strength of 185.0 MPa

H19

EN 573-3

Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H19

EN 573-3

Flat

Thermal conductivity

200 W/(m·K)

Show Material materials with Thermal conductivity of 200 W/(m·K)

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

201 W/(m·K)

Show Material materials with Thermal conductivity of 201 W/(m·K)

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

H19

EN 573-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

30000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 S/m

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Electrical resistivity

3.33e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 Ω·m

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

H19

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Flat, Coil, Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H19

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.1 %

Show Material materials with Chromium of 0.1 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Copper

0.2 %

Show Material materials with Copper of 0.2 %

H19

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.2 %

Show Material materials with Copper of 0.2 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H19

EN 573-3

Flat

0.70 %

Show Material materials with Iron of 0.70 %

H19

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.7 %

Show Material materials with Iron of 0.7 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Magnesium

0.5 - 1.1 %

Show Material materials with Magnesium of 0.5 - 1.1 %

H19

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar, Coil, Sheet, Strip

Manganese

0.2 %

Show Material materials with Manganese of 0.2 %

H19

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.2 %

Show Material materials with Manganese of 0.2 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H19

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.3 %

Show Material materials with Silicon of 0.3 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H19

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.25 %

Show Material materials with Zinc of 0.25 %

H19

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Heat exchangers: Fins, General applications; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim; Components: Automotive fins, Heat exchangers

Brazing

hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability