EN 573-3 Grade AW-5005A O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.68 g/cm³

Show Material materials with Density of 2.68 g/cm³

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.69 - 2.7 g/cm³

Show Material materials with Density of 2.69 - 2.7 g/cm³

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3

Profile, Rod, Flat, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

Elastic modulus

60.0 GPa

Show Material materials with Elastic modulus of 60.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3

Profile, Rod, Flat, Tube

Elongation

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Bar

A100

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

A50

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

A50

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Tube, Bar

A100

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

A50

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Flat

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Rod, Tube

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Flat

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Flat

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Profile, Tube, Rod, Flat

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Flat

A50

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Bar

20.0 °C

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3

Flat

20.0 °C

30.0 [-]

Show Material materials with Hardness, Brinell of 30.0 [-]

O

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Profile, Rod, Flat, Tube

Shear modulus

23.8 GPa

Show Material materials with Shear modulus of 23.8 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

20.0 °C

25.0 - 26.1 GPa

Show Material materials with Shear modulus of 25.0 - 26.1 GPa

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3

Profile, Rod, Flat, Tube

Tensile strength

20.0 °C

100.0 - 150.0 MPa

Show Material materials with Tensile strength of 100.0 - 150.0 MPa

O

EN 573-3, EN 755

Profile, Rod, Tube, Strip, Sheet, Plate, Bar

20.0 °C

100.0 - 145.0 MPa

Show Material materials with Tensile strength of 100.0 - 145.0 MPa

O

EN 573-3, EN 485, EN 754

Rod, Tube, Flat, Strip, Sheet, Plate, Bar

20.0 °C

100.0 - 145.0 MPa

Show Material materials with Tensile strength of 100.0 - 145.0 MPa

O

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

-50.0 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

20 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

100.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20-100°C

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

200.0 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

300 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

300.0 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 650.0 °C

Show Material materials with Melting point of 630.0 - 650.0 °C

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

20.0 °C

879.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 J/(kg·K)

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

879.0 - 899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 899.0 J/(kg·K)

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

O

EN 573-3

Profile, Rod, Flat, Tube

Thermal conductivity

168.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 168.0 - 190.0 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20.0 °C

160.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 220.0 W/(m·K)

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat

20.0 °C

160.0 - 201.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 201.0 W/(m·K)

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

201.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 - 220.0 W/(m·K)

O

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

O

EN 573-3

Profile, Rod, Flat, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

23000000.0 - 31000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 31000000.0 S/m

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

Electrical resistivity

3.23e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 - 4.35e-08 Ω·m

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Tube, Bar

3.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.5e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

O

EN 573-3

Profile, Rod, Flat, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Copper

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Iron

0.45 %

Show Material materials with Iron of 0.45 %

O

EN 573-3

Profile, Rod, Flat, Tube

0.45 %

Show Material materials with Iron of 0.45 %

O

EN 573-3, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Tube, Bar, Coil, Sheet, Strip

Magnesium

0.7 - 1.1 %

Show Material materials with Magnesium of 0.7 - 1.1 %

O

EN 573-3, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar, Coil, Sheet, Strip

Manganese

0.15 %

Show Material materials with Manganese of 0.15 %

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.15 %

Show Material materials with Manganese of 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Other

0.05 - 0.15 %

Show Material materials with Other of 0.05 - 0.15 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

O

EN 573-3, EN 485, EN 754, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent (anodizing quality)

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Heat exchangers: Fins; Cosmetics: Cosmetics pieces; Pharmacy: Pharma and para-Pharma; Automotive Trim: Interior Trim, Windows frames; Components: Automotive fins, Heat exchangers

Brazing

Good

Corrosion properties

Excellent

Welding

Excellent

Workability

Good