General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Density | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
2.69 g/cm³ Show Material materials with Density of 2.69 g/cm³ | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Elongation | 10.0 % Show Material materials with Elongation of 10.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | |
12.0 % Show Material materials with Elongation of 12.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | H112 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | H112 | EN 573-3 | Flat | A50 | |
Hardness, Brinell | 39.0 [-] Show Material materials with Hardness, Brinell of 39.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 39.0 [-] Show Material materials with Hardness, Brinell of 39.0 [-] | H112 | EN 573-3 | Flat, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 26.0 - 26.5 GPa Show Material materials with Shear modulus of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Tensile strength | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | H112 | EN 573-3 | Sheet, Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 620.0 - 650.0 °C Show Material materials with Melting point of 620.0 - 650.0 °C | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
625.0 - 650.0 °C Show Material materials with Melting point of 625.0 - 650.0 °C | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Specific heat capacity | 879.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Thermal conductivity | 170.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 190.0 W/(m·K) | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
193 W/(m·K) Show Material materials with Thermal conductivity of 193 W/(m·K) | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Electrical
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Electrical conductivity | 23000000.0 - 26000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
29000000.0 S/m Show Material materials with Electrical conductivity of 29000000.0 S/m | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Electrical resistivity | 3.45e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 Ω·m | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Copper | 0.2 % Show Material materials with Copper of 0.2 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | H112 | EN 573-3 | Flat, Sheet |
0.70 % Show Material materials with Iron of 0.70 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Magnesium | 1.1 - 1.8 % Show Material materials with Magnesium of 1.1 - 1.8 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
0.3 % Show Material materials with Manganese of 0.3 % | H112 | EN 573-3 | Flat, Sheet | |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H112 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |