The high-strength material has a high fracture toughness also for larger thicknesses and resistance to stress corrosion also in the ST direction and exfoliation corrosion. It has a low distortion post machining. Application: integral and fittings of larger dimensions

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.82 g/cm³

Show Material materials with Density of 2.82 g/cm³

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Elongation

9.0 %

Show Material materials with Elongation of 9.0 %

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

T7452

WL 3.4394

Forging

Hardness, Brinell

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

20.0 °C

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T7452

WL 3.4394

Forging

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

27.0 GPa

Show Material materials with Shear modulus of 27.0 GPa

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Tensile strength

480.0 MPa

Show Material materials with Tensile strength of 480.0 MPa

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

495.0 MPa

Show Material materials with Tensile strength of 495.0 MPa

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

20.0 °C

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T7452

WL 3.4394

Forging

20.0 °C

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T7452

WL 3.4394

Forging

20.0 °C

475.0 MPa

Show Material materials with Tensile strength of 475.0 MPa

T7452

WL 3.4394

Forging

20.0 °C

480.0 MPa

Show Material materials with Tensile strength of 480.0 MPa

T7452

WL 3.4394

Forging

20.0 °C

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T7452

WL 3.4394

Forging

20.0 °C

495.0 MPa

Show Material materials with Tensile strength of 495.0 MPa

T7452

WL 3.4394

Forging

Thermal

PropertyValueComment

Coefficient of thermal expansion

2.1e-05 - 2.4e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 - 2.4e-05 1/K

Typical for Wrought 7000 Series Aluminium

Melting point

465.0 - 655.0 °C

Show Material materials with Melting point of 465.0 - 655.0 °C

Typical for Wrought 7000 Series Aluminium

Specific heat capacity

795.0 - 1050.0 J/(kg·K)

Show Material materials with Specific heat capacity of 795.0 - 1050.0 J/(kg·K)

Typical for Wrought 7000 Series Aluminium

Thermal conductivity

121.0 - 170.0 W/(m·K)

Show Material materials with Thermal conductivity of 121.0 - 170.0 W/(m·K)

Typical for Wrought 7000 Series Aluminium

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Electrical resistivity

4e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 %

Show Material materials with Chromium of 0.05 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Copper

1.5 - 2.0 %

Show Material materials with Copper of 1.5 - 2.0 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Iron

0.15 %

Show Material materials with Iron of 0.15 %

T7452

WL 3.4394

Forging

0.15 %

Show Material materials with Iron of 0.15 %

T7452

WL 3.4394

Sheet, Strip, Bar, Wire

Magnesium

2.1 - 2.6 %

Show Material materials with Magnesium of 2.1 - 2.6 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Nickel

0.05 %

Show Material materials with Nickel of 0.05 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Silicon

0.12 %

Show Material materials with Silicon of 0.12 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Titanium

0.06 %

Show Material materials with Titanium of 0.06 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Zinc

5.7 - 6.7 %

Show Material materials with Zinc of 5.7 - 6.7 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Zirconium

0.1 - 0.16 %

Show Material materials with Zirconium of 0.1 - 0.16 %

T7452

WL 3.4394

Forging, Sheet, Strip, Bar, Wire

Technological properties

Property
Brazing

Excellent