EN AW-2014 is an alloy with strength, machinability and welding capabilities, Aluminum Alloy EN AW-2014 is an excellent option. It is a precipitation hardening alloy that maintains strength after heat treatment.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T652

EN 573-3

Forging

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T652

EN 573-3

Forging

Elongation

2.0 %

Show Material materials with Elongation of 2.0 %

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

A100

3.0 %

Show Material materials with Elongation of 3.0 %

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

T652

EN 573-3

Forging

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

T652

EN 573-3

Forging

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

T652

EN 573-3

Forging

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

T652

EN 573-3

Forging

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

T652

EN 573-3

Forging

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

T652

EN 573-3

Forging

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

T652

EN 573-3

A50 Transverse

Plane-Strain Fracture Toughnes

20.0 °C

19.9 - 31.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 19.9 - 31.6 MPa·√m

T652

EN 573-3

20.0 °C

19.9 - 24.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 19.9 - 24.0 MPa·√m

T652

EN 573-3

20.0 °C

19.9 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 19.9 MPa·√m

T652

EN 573-3

20.0 °C

24.0 - 31.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 31.6 MPa·√m

T652

EN 573-3

20.0 °C

24.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 24.0 MPa·√m

T652

EN 573-3

20.0 °C

31.6 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 31.6 MPa·√m

T652

EN 573-3

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Shear modulus

27.4 GPa

Show Material materials with Shear modulus of 27.4 GPa

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

Tensile strength

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T652

EN 573-3

Transverse

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T652

EN 573-3

Transverse

20.0 °C

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T652

EN 573-3

Forging

20.0 °C

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T652

EN 573-3

Forging

20.0 °C

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T652

EN 573-3

Forging

20.0 °C

430.0 MPa

Show Material materials with Tensile strength of 430.0 MPa

T652

EN 573-3

Forging

20.0 °C

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T652

EN 573-3

Forging

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

-50.0 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.1e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

100 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

100.0 °C

2.28e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

100 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

200 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

200.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

300 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

300.0 °C

2.46e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

Melting point

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

510.0 - 640.0 °C

Show Material materials with Melting point of 510.0 - 640.0 °C

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

Specific heat capacity

816.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K)

Typical for Wrought 2000 Series Aluminium

Thermal conductivity

134.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K)

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

140.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 200.0 W/(m·K)

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

21000000.0 - 24000000.0 S/m

Show Material materials with Electrical conductivity of 21000000.0 - 24000000.0 S/m

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

20.0 °C

20000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

3.45e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

4.17e-08 - 4.76e-08 Ω·m

Show Material materials with Electrical resistivity of 4.17e-08 - 4.76e-08 Ω·m

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Iron

0.7 %

Show Material materials with Iron of 0.7 %

T652

EN 573-3

Forging

0.70 %

Show Material materials with Iron of 0.70 %

T652

EN 573-3, EN 586

Strip, Sheet, Plate, Forging, Tube, Bar

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Silicon

0.5 - 1.2 %

Show Material materials with Silicon of 0.5 - 1.2 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T652

EN 573-3, EN 586

Forging, Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable