EN 573-3 Grade AW-1350 F

Want to keep this datasheet? Save it now in your required format

Description

Material EN AW-EAl 99,5 is produced in high amount for wire and prewire for electrotechnical applications as well as for extruded components and drawn parts. The alloy is food-safe.

Related Standards

Equivalent Materials

This material data has been provided by AluKey,WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

2.705 g/cm³

Show Material materials with Density of 2.705 g/cm³

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Elongation

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3, EN 755

Plate, Rod

A50

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3, EN 755

Plate, Rod

A100

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

F

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

F

EN 573-3

Profile, Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

Typical for Wrought 1000 Series Aluminium

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3, EN 485, EN 755

Plate, Rod

65.0 MPa

Show Material materials with Tensile strength of 65.0 MPa

F

EN 573-3, EN 14121

Plate, Rod

20.0 °C

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

F

EN 573-3

Profile, Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Unlock all property charts

Melting point

645.0 - 657.0 °C

Show Material materials with Melting point of 645.0 - 657.0 °C

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Specific heat capacity

900.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K)

Typical for Wrought 1000 Series Aluminium

Thermal conductivity

225.0 - 235.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 - 235.0 W/(m·K)

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

234 W/(m·K)

Show Material materials with Thermal conductivity of 234 W/(m·K)

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

35400000.0 - 36500000.0 S/m

Show Material materials with Electrical conductivity of 35400000.0 - 36500000.0 S/m

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

36000000.0 S/m

Show Material materials with Electrical conductivity of 36000000.0 S/m

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Electrical resistivity

2.74e-08 - 2.82e-08 Ω·m

Show Material materials with Electrical resistivity of 2.74e-08 - 2.82e-08 Ω·m

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

2.78e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 Ω·m

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

Boron

0.05 %

Show Material materials with Boron of 0.05 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Chromium

0.01 %

Show Material materials with Chromium of 0.01 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Copper

0.05 %

Show Material materials with Copper of 0.05 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Iron

0.40 %

Show Material materials with Iron of 0.40 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod

0.4 %

Show Material materials with Iron of 0.4 %

F

EN 573-3

Profile, Rod, Tube

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

F

EN 573-3, EN 14121, EN 485, EN 755

Plate, Rod, Profile, Tube

Technological properties

Property
Brazing

Excellent

Workability

Excellent workability.