EN 573-3 Grade AW-1050A H14

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

25.0 MPa

Show Material materials with Bending Fatigue Strength of 25.0 MPa

H14

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

35.0 MPa

Show Material materials with Bending Fatigue Strength of 35.0 MPa

H14

EN 573-3, EN 1301, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

-195.0 °C

78.4 GPa

Show Material materials with Elastic modulus of 78.4 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

-85.0 °C

73.5 GPa

Show Material materials with Elastic modulus of 73.5 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

-30.0 °C

71.4 GPa

Show Material materials with Elastic modulus of 71.4 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

100.0 °C

68.0 - 68.6 GPa

Show Material materials with Elastic modulus of 68.0 - 68.6 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

100.0 °C

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

150.0 °C

66.0 - 66.5 GPa

Show Material materials with Elastic modulus of 66.0 - 66.5 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

150.0 °C

66.5 GPa

Show Material materials with Elastic modulus of 66.5 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

250.0 °C

56.0 - 57.0 GPa

Show Material materials with Elastic modulus of 56.0 - 57.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

250.0 °C

56.0 GPa

Show Material materials with Elastic modulus of 56.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Foil

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Foil

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Foil, Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Foil

A100

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Wire

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Flat

Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Rod, Tube, Flat

Hardness, Brinell

34.0 [-]

Show Material materials with Hardness, Brinell of 34.0 [-]

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

30.0 [-]

Show Material materials with Hardness, Brinell of 30.0 [-]

H14

EN 573-3

Rod, Tube

20.0 °C

34.0 [-]

Show Material materials with Hardness, Brinell of 34.0 [-]

H14

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

25.0 - 25.9 GPa

Show Material materials with Shear modulus of 25.0 - 25.9 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

25.9 - 26.5 GPa

Show Material materials with Shear modulus of 25.9 - 26.5 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Tensile strength

100.0 MPa

Show Material materials with Tensile strength of 100.0 MPa

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

100.0 - 135.0 MPa

Show Material materials with Tensile strength of 100.0 - 135.0 MPa

H14

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

20.0 °C

100.0 MPa

Show Material materials with Tensile strength of 100.0 MPa

H14

EN 573-3

Wire

20.0 °C

105.0 - 145.0 MPa

Show Material materials with Tensile strength of 105.0 - 145.0 MPa

H14

EN 573-3

Flat

Transverse

20.0 °C

105.0 - 145.0 MPa

Show Material materials with Tensile strength of 105.0 - 145.0 MPa

H14

EN 573-3, EN 485, EN 683

Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Melting point

646.0 - 657.0 °C

Show Material materials with Melting point of 646.0 - 657.0 °C

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

899.0 - 900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 - 900.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

899.0 J/(kg·K)

Show Material materials with Specific heat capacity of 899.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Thermal conductivity

20.0 °C

210.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K)

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20.0 °C

210.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 229.0 W/(m·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

220.0 - 229.0 W/(m·K)

Show Material materials with Thermal conductivity of 220.0 - 229.0 W/(m·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

229.0 W/(m·K)

Show Material materials with Thermal conductivity of 229.0 W/(m·K)

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

34000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34000000.0 - 36000000.0 S/m

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34800000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 34800000.0 - 36000000.0 S/m

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Electrical resistivity

2.78e-08 - 2.94e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.94e-08 Ω·m

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.8e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 2.9e-08 Ω·m

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

20.0 °C

2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.9e-08 Ω·m

H14

EN 573-3

Rod, Flat, Foil, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Boron

0.05

Show Material materials with Boron of 0.05

H14

EN 573-3

Flat

Chromium

0.01

Show Material materials with Chromium of 0.01

H14

EN 573-3

Flat

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Gallium

0.03

Show Material materials with Gallium of 0.03

H14

EN 573-3

Flat

Iron

0.4 %

Show Material materials with Iron of 0.4 %

H14

EN 573-3

Flat, Rod, Foil, Tube, Wire

0.40 %

Show Material materials with Iron of 0.40 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

H14

EN 573-3

Flat

0.05 %

Show Material materials with Magnesium of 0.05 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Manganese

0.01 %

Show Material materials with Manganese of 0.01 %

H14

EN 573-3

Flat

0.05 %

Show Material materials with Manganese of 0.05 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Nickel

0.03

Show Material materials with Nickel of 0.03

H14

EN 573-3

Flat

Silicon

0.1 %

Show Material materials with Silicon of 0.1 %

H14

EN 573-3

Flat

0.25 %

Show Material materials with Silicon of 0.25 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

H14

EN 573-3

Flat

0.05 %

Show Material materials with Titanium of 0.05 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Vanadium

0.03

Show Material materials with Vanadium of 0.03

H14

EN 573-3

Flat

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H14

EN 573-3

Flat

0.07 %

Show Material materials with Zinc of 0.07 %

H14

EN 573-3, EN 1301, EN 485, EN 683, EN 754

Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: acceptable, weathering: good

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12)