EN 573-3 Grade AW-1060

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueRelated StandardsShape

Density

2.705 g/cm³

Show Material materials with Density of 2.705 g/cm³

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Mechanical

PropertyValueRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

Typical for Wrought 1000 Series Aluminium

Thermal

PropertyTemperatureValueRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

EN 573-3

Strip, Sheet, Plate, Tube, Bar

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Specific heat capacity

900.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K)

Typical for Wrought 1000 Series Aluminium

Thermal conductivity

230.0 - 234.0 W/(m·K)

Show Material materials with Thermal conductivity of 230.0 - 234.0 W/(m·K)

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Electrical

PropertyValueRelated StandardsShape

Electrical conductivity

35000000.0 - 36000000.0 S/m

Show Material materials with Electrical conductivity of 35000000.0 - 36000000.0 S/m

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Electrical resistivity

2.78e-08 - 2.86e-08 Ω·m

Show Material materials with Electrical resistivity of 2.78e-08 - 2.86e-08 Ω·m

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Chemical properties

PropertyValueRelated StandardsShape

Aluminium

99.6 %

Show Material materials with Aluminium of 99.6 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Iron

0.35 %

Show Material materials with Iron of 0.35 %

EN 573-3

0.35 %

Show Material materials with Iron of 0.35 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Magnesium

0.03 %

Show Material materials with Magnesium of 0.03 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Titanium

0.03 %

Show Material materials with Titanium of 0.03 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Vanadium

0.05 %

Show Material materials with Vanadium of 0.05 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

EN 573-3

Strip, Sheet, Plate, Tube, Bar

Technological properties

Property
Brazing

Excellent

Workability

Excellent workability.