EN 573-3 Grade AW-1080A H12

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H12

EN 573-3

Flat

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet, Strip

3 mm

Show Material materials with Thickness of 3 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

3 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

1 °/t

Show Material materials with Bending angle 180° of 1 °/t

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Bending angle 90°

1 °/t

Show Material materials with Bending angle 90° of 1 °/t

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Elastic modulus

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H12

EN 573-3

Flat

-270.0 °C, 20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Coil, Sheet, Strip

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H12

EN 573-3

Flat

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H12

EN 573-3

Flat

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H12

EN 573-3

Flat

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H12

EN 573-3

Flat

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H12

EN 573-3

Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H12

EN 573-3

Flat

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Hardness, Brinell

20.0 °C

26.0 [-]

Show Material materials with Hardness, Brinell of 26.0 [-]

H12

EN 573-3

Flat

26.0 [-]

Show Material materials with Hardness, Brinell of 26.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Hardness, HBW

26.0 - 36.0 [-]

Show Material materials with Hardness, HBW of 26.0 - 36.0 [-]

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 GPa

Show Material materials with Shear modulus of 25.0 GPa

H12

EN 573-3

Flat

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Tensile strength

20.0 °C

80.0 - 120.0 MPa

Show Material materials with Tensile strength of 80.0 - 120.0 MPa

H12

EN 573-3

Flat

Transverse

80.0 - 150.0 MPa

Show Material materials with Tensile strength of 80.0 - 150.0 MPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

20.0 °C

80.0 - 120.0 MPa

Show Material materials with Tensile strength of 80.0 - 120.0 MPa

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire, Flat

Unlock all property charts

Yield strength

20.0 °C

55.0 MPa

Show Material materials with Yield strength of 55.0 MPa

H12

EN 573-3

Flat

RP02 Transverse

55.0 MPa

Show Material materials with Yield strength of 55.0 MPa

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

RP02

20.0 °C

55.0 MPa

Show Material materials with Yield strength of 55.0 MPa

H12

EN 573-3

Flat

RP02

55.0 - 90.0 MPa

Show Material materials with Yield strength of 55.0 - 90.0 MPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

according to EN 485-2

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000023 1/K

Show Material materials with Coefficient of thermal expansion of 0.000023 1/K

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20-100°C

100 °C, 20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Unlock all property charts

Melting point

659.0 °C

Show Material materials with Melting point of 659.0 °C

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

H12

EN 573-3

Flat

Thermal conductivity

20.0 °C

215.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 W/(m·K)

H12

EN 573-3

Flat

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

225 W/(m·K)

Show Material materials with Thermal conductivity of 225 W/(m·K)

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

36400000.0 - 37000000.0 S/m

Show Material materials with Electrical conductivity of 36400000.0 - 37000000.0 S/m

H12

EN 573-3

Flat

34500000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35000000.0 S/m

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Electrical resistivity

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

2.86e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.86e-08 - 2.9e-08 Ω·m

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Wire

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.8 %

Show Material materials with Aluminium of 99.8 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

Copper

0.03 %

Show Material materials with Copper of 0.03 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

0.03 %

Show Material materials with Copper of 0.03 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

Iron

0.15 %

Show Material materials with Iron of 0.15 %

H12

EN 573-3

Flat

0.15 %

Show Material materials with Iron of 0.15 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3, EN 485

Coil, Sheet, Strip, Strip, Sheet, Plate, Wire

Magnesium

0.02 %

Show Material materials with Magnesium of 0.02 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

0.02 %

Show Material materials with Magnesium of 0.02 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Manganese

0.02 %

Show Material materials with Manganese of 0.02 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

0.02 %

Show Material materials with Manganese of 0.02 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Other

0.02 %

Show Material materials with Other of 0.02 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Min.

Silicon

0.15 %

Show Material materials with Silicon of 0.15 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

0.15 %

Show Material materials with Silicon of 0.15 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Titanium

0.02 %

Show Material materials with Titanium of 0.02 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

Zinc

0.06 %

Show Material materials with Zinc of 0.06 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Wire

0.06 %

Show Material materials with Zinc of 0.06 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetic pieces; Automotive trim: Interior trim, Windows frame, Marque badges

Brazing

Excellent

Corrosion properties

Excellent

Welding

Excellent

Workability

Excellent