EN 573-3 Grade AW-1098 O

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3

Rod, Sheet, Strip, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

20.0 °C

70.0 - 72.0 GPa

Show Material materials with Elastic modulus of 70.0 - 72.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

20.0 °C

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

O

EN 573-3

Wire

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

O

EN 573-3

Wire, Rod, Sheet, Strip

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Wire, Rod

Elongation

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3, EN 1301

Strip, Sheet, Plate

29.0 %

Show Material materials with Elongation of 29.0 %

O

EN 573-3

Strip, Sheet, Plate

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

Strip, Sheet, Plate

33.0 %

Show Material materials with Elongation of 33.0 %

O

EN 573-3

Strip, Sheet, Plate

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3

Wire

A100

20.0 °C

29.0 %

Show Material materials with Elongation of 29.0 %

O

EN 573-3

Rod

20.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

Sheet, Strip

20.0 °C

33.0 %

Show Material materials with Elongation of 33.0 %

O

EN 573-3

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

O

EN 573-3

Rod, Sheet, Strip, Wire

Tensile strength

40.0 MPa

Show Material materials with Tensile strength of 40.0 MPa

O

EN 573-3

Strip, Sheet, Plate

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20.0 °C

40.0 MPa

Show Material materials with Tensile strength of 40.0 MPa

O

EN 573-3

Rod, Sheet, Strip

20.0 °C

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3

Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

-50.0 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

20 °C

2.18e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

20 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate

100.0 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3

Rod, Sheet, Strip, Wire

200 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

200.0 °C

2.45e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

300 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

300.0 °C

2.55e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.55e-05 1/K

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Rod, Wire

Melting point

660.0 °C

Show Material materials with Melting point of 660.0 °C

O

EN 573-3, EN 1301

Strip, Sheet, Plate

Specific heat capacity

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20.0 °C

900.0 J/(kg·K)

Show Material materials with Specific heat capacity of 900.0 J/(kg·K)

O

EN 573-3

Rod, Sheet, Strip, Wire

Thermal conductivity

232 W/(m·K)

Show Material materials with Thermal conductivity of 232 W/(m·K)

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20.0 °C

215.0 - 227.0 W/(m·K)

Show Material materials with Thermal conductivity of 215.0 - 227.0 W/(m·K)

O

EN 573-3

Rod, Sheet, Strip, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

37500000.0 - 37700000.0 S/m

Show Material materials with Electrical conductivity of 37500000.0 - 37700000.0 S/m

O

EN 573-3, EN 1301

Strip, Sheet, Plate

20.0 °C

37600000.0 - 37800000.0 S/m

Show Material materials with Electrical conductivity of 37600000.0 - 37800000.0 S/m

O

EN 573-3

Rod, Sheet, Strip, Wire

Electrical resistivity

2.65e-08 - 2.67e-08 Ω·m

Show Material materials with Electrical resistivity of 2.65e-08 - 2.67e-08 Ω·m

O

EN 573-3, EN 1301

Strip, Sheet, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.98 %

Show Material materials with Aluminium of 99.98 %

O

EN 573-3, EN 1301

Rod, Sheet, Strip, Wire, Plate

Copper

0.003 %

Show Material materials with Copper of 0.003 %

O

EN 573-3, EN 1301

Rod, Sheet, Strip, Wire, Plate

Iron

0.006 %

Show Material materials with Iron of 0.006 %

O

EN 573-3

Rod, Sheet, Strip, Wire

0.006 %

Show Material materials with Iron of 0.006 %

O

EN 573-3, EN 1301

Strip, Sheet, Plate

Silicon

0.01 %

Show Material materials with Silicon of 0.01 %

O

EN 573-3, EN 1301

Rod, Sheet, Strip, Wire, Plate

Titanium

0.003 %

Show Material materials with Titanium of 0.003 %

O

EN 573-3, EN 1301

Rod, Sheet, Strip, Wire, Plate

Zinc

0.015 %

Show Material materials with Zinc of 0.015 %

O

EN 573-3, EN 1301

Rod, Sheet, Strip, Wire, Plate

Technological properties

Property
Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good, general: very good

Corrosion properties

Seawater: acceptable, weathering: good

Workability

Bending / Spinning (cold): very good