EN 573-3 Grade AW-1200 H16

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

2.71 - 2.72 g/cm³

Show Material materials with Density of 2.71 - 2.72 g/cm³

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H16

EN 573-3

Rod, Flat, Foil, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H16

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H16

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H16

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastic modulus of 60.0 - 65.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastic modulus of 65.0 - 69.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H16

EN 573-3, EN 485, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H16

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H16

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H16

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H16

EN 573-3

Foil, Flat

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H16

EN 573-3

Flat

A50 Transverse

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H16

EN 573-3

Foil

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H16

EN 573-3

Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H16

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H16

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H16

EN 573-3

Rod, Tube

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H16

EN 573-3

Flat

A50 Transverse

Hardness, Brinell

42.0 [-]

Show Material materials with Hardness, Brinell of 42.0 [-]

H16

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

35.0 [-]

Show Material materials with Hardness, Brinell of 35.0 [-]

H16

EN 573-3

Rod, Tube

20.0 °C

42.0 [-]

Show Material materials with Hardness, Brinell of 42.0 [-]

H16

EN 573-3

Flat

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

H16

EN 573-3

Rod, Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H16

EN 573-3

Rod, Flat, Foil, Tube

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

24.0 - 26.0 GPa

Show Material materials with Shear modulus of 24.0 - 26.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

24.0 - 25.9 GPa

Show Material materials with Shear modulus of 24.0 - 25.9 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

25.9 - 26.0 GPa

Show Material materials with Shear modulus of 25.9 - 26.0 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H16

EN 573-3

Rod, Flat, Foil, Tube

Tensile strength

20.0 °C

120.0 - 170.0 MPa

Show Material materials with Tensile strength of 120.0 - 170.0 MPa

H16

EN 573-3, EN 683

Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube

20.0 °C

120.0 - 170.0 MPa

Show Material materials with Tensile strength of 120.0 - 170.0 MPa

H16

EN 573-3

Flat

Transverse

20.0 °C

125.0 - 180.0 MPa

Show Material materials with Tensile strength of 125.0 - 180.0 MPa

H16

EN 573-3

Foil

20.0 °C

130.0 - 170.0 MPa

Show Material materials with Tensile strength of 130.0 - 170.0 MPa

H16

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

130.0 - 170.0 MPa

Show Material materials with Tensile strength of 130.0 - 170.0 MPa

H16

EN 573-3

Flat

Transverse

20.0 °C

135.0 - 170.0 MPa

Show Material materials with Tensile strength of 135.0 - 170.0 MPa

H16

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H16

EN 573-3

Rod, Flat, Foil, Tube

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H16

EN 573-3

Rod, Flat, Foil, Tube

Melting point

644.0 - 657.0 °C

Show Material materials with Melting point of 644.0 - 657.0 °C

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H16

EN 573-3

Rod, Flat, Foil, Tube

Thermal conductivity

20.0 °C

205.0 - 210.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K)

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

205.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 225.0 W/(m·K)

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

210.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 225.0 W/(m·K)

H16

EN 573-3

Rod, Flat, Foil, Tube

20.0 °C

225.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 W/(m·K)

H16

EN 573-3

Rod, Flat, Foil, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

33000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34400000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m

H16

EN 573-3

Rod, Flat, Foil, Tube

Electrical resistivity

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m

H16

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.95e-08 Ω·m

Show Material materials with Electrical resistivity of 2.95e-08 Ω·m

H16

EN 573-3

Rod, Flat, Foil, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.0 %

Show Material materials with Aluminium of 99.0 %

H16

EN 573-3, EN 485, EN 683, EN 754

Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H16

EN 573-3, EN 485, EN 683, EN 754

Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

H16

EN 573-3, EN 485, EN 683, EN 754

Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

H16

EN 573-3, EN 485, EN 683, EN 754

Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H16

EN 573-3, EN 485, EN 683, EN 754

Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12)