EN 573-3 Grade AW-1200 H18

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

2.71 - 2.72 g/cm³

Show Material materials with Density of 2.71 - 2.72 g/cm³

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H18

EN 573-3

Foil, Rod, Flat, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

0.2 mm

Coil, Sheet, Foil

3.0 mm

Show Material materials with Thickness of 3.0 mm

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

3.0 mm

Coil, Sheet, Foil

40 mm

Show Material materials with Thickness of 40 mm

H18

EN 546-2, EN 573-1, EN 573-2, EN 573-3, En 485-2

40 mm

Coil, Sheet, Foil

200 mm

Show Material materials with Thickness of 200 mm

H18

EN 546-2, EN 573-1, EN 573-2, EN 573-3, En 485-2

200 mm

Coil, Sheet, Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

65.0 MPa

Show Material materials with Bending Fatigue Strength of 65.0 MPa

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

3.0 °/t

Show Material materials with Bending angle 90° of 3.0 °/t

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

3 °/t

Show Material materials with Bending angle 90° of 3 °/t

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastic modulus of 60.0 - 65.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastic modulus of 65.0 - 69.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

1 %

Show Material materials with Elongation of 1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Foil

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Foil, Flat

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H18

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H18

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3

Rod, Tube

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H18

EN 573-3

Rod, Tube

Hardness, Brinell

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

H18

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

43.0 [-]

Show Material materials with Hardness, Brinell of 43.0 [-]

H18

EN 573-3

Rod, Tube

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

H18

EN 573-3

Flat

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

H18

EN 573-3

Rod, Tube

Hardness, HBW

31.0 - 45.0 [-]

Show Material materials with Hardness, HBW of 31.0 - 45.0 [-]

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H18

EN 573-3

Foil, Rod, Flat, Tube

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

20.0 °C

24.0 - 26.0 GPa

Show Material materials with Shear modulus of 24.0 - 26.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

24.0 - 25.9 GPa

Show Material materials with Shear modulus of 24.0 - 25.9 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

25.9 - 26.0 GPa

Show Material materials with Shear modulus of 25.9 - 26.0 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H18

EN 573-3

Foil, Rod, Flat, Tube

Tensile strength

95.0 - 150.0 MPa

Show Material materials with Tensile strength of 95.0 - 150.0 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

140.0 MPa

Show Material materials with Tensile strength of 140.0 MPa

H18

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

H18

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

140.0 MPa

Show Material materials with Tensile strength of 140.0 MPa

H18

EN 573-3

Foil

20.0 °C

140.0 - 200.0 MPa

Show Material materials with Tensile strength of 140.0 - 200.0 MPa

H18

EN 573-3, EN 546, EN 546-2, EN 573-1, EN 573-2, EN 573-3, En 485-2

Foil, Strip, Sheet, Plate, Bar, Rod, Tube, Coil, Sheet, Foil

20.0 °C

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

H18

EN 573-3

Rod, Tube, Flat

20.0 °C

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

H18

EN 573-3

Flat

Transverse

Yield strength

75.0 - 130.0 MPa

Show Material materials with Yield strength of 75.0 - 130.0 MPa

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2

Coil, Sheet, Foil

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H18

EN 573-3, EN 485, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

20.0 °C

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H18

EN 573-3

Rod, Foil, Flat

RP02

20.0 °C

130.0 MPa

Show Material materials with Yield strength of 130.0 MPa

H18

EN 573-3

Flat

RP02 Transverse

20.0 °C

135.0 MPa

Show Material materials with Yield strength of 135.0 MPa

H18

EN 573-3

Foil

RP02

20.0 °C

150.0 MPa

Show Material materials with Yield strength of 150.0 MPa

H18

EN 573-3

Tube

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

-50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

20-100°C

200 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H18

EN 573-3

Foil, Rod, Flat, Tube

300 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H18

EN 573-3

Foil, Rod, Flat, Tube

Melting point

644.0 - 657.0 °C

Show Material materials with Melting point of 644.0 - 657.0 °C

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H18

EN 573-3

Foil, Rod, Flat, Tube

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

20.0 °C

205.0 - 210.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K)

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat

20.0 °C

205.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 225.0 W/(m·K)

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

210.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 225.0 W/(m·K)

H18

EN 573-3

Foil, Rod, Flat, Tube

20.0 °C

225.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 W/(m·K)

H18

EN 573-3

Foil, Rod, Flat, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

33000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

34400000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m

H18

EN 573-3

Foil, Rod, Flat, Tube

Electrical resistivity

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

20.0 °C

2.95e-08 Ω·m

Show Material materials with Electrical resistivity of 2.95e-08 Ω·m

H18

EN 573-3

Foil, Rod, Flat, Tube

Chemical properties

PropertyValueConditionRelated StandardsShapeComment

Aluminium

99.0 %

Show Material materials with Aluminium of 99.0 %

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.05 %

Show Material materials with Copper of 0.05 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Iron

1 %

Show Material materials with Iron of 1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Si + Fe

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.05 %

Show Material materials with Manganese of 0.05 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Other

0.15 %

Show Material materials with Other of 0.15 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Silicon

1 %

Show Material materials with Silicon of 1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Si + Fe

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.05 %

Show Material materials with Titanium of 0.05 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H18

EN 573-3, EN 485, EN 546, EN 683, EN 754

Foil, Rod, Flat, Tube, Strip, Sheet, Plate, Bar

0.1 %

Show Material materials with Zinc of 0.1 %

H18

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 546-2, En 485-2

Coil, Sheet, Foil

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins; Cable wrapping: Electric cable wrapping; Insulation; Solar: Solar collectors; Semi-rigid and corrugated: Smooth wall

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Welding

Excellent

Workability