EN 573-3 Grade AW-1200 H112

Want to keep this datasheet? Save it now in your required format

Description

Food safe aluminum.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.71 - 2.72 g/cm³

Show Material materials with Density of 2.71 - 2.72 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H112

EN 573-3

Profile, Rod, Flat, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastic modulus of 60.0 - 65.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastic modulus of 65.0 - 69.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

Unlock all property charts

Elongation

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

H112

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Flat

A50

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

18.0 %

Show Material materials with Elongation of 18.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Flat

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3

Flat

Transverse

16.0 %

Show Material materials with Elongation of 16.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

20.0 %

Show Material materials with Elongation of 20.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

Unlock all property charts

Hardness, Brinell

20.0 °C

23.0 [-]

Show Material materials with Hardness, Brinell of 23.0 [-]

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

26.0 [-]

Show Material materials with Hardness, Brinell of 26.0 [-]

H112

EN 573-3

Flat

20.0 °C

24.0 - 26.0 [-]

Show Material materials with Hardness, Brinell of 24.0 - 26.0 [-]

H112

EN 573-3

Flat

20.0 °C

24.0 [-]

Show Material materials with Hardness, Brinell of 24.0 [-]

H112

EN 573-3

Flat

26.0 [-]

Show Material materials with Hardness, Brinell of 26.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

24.0 [-]

Show Material materials with Hardness, Brinell of 24.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Unlock all property charts

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H112

EN 573-3

Profile, Rod, Flat, Tube

Shear modulus

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

24.0 - 26.0 GPa

Show Material materials with Shear modulus of 24.0 - 26.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

25.9 - 26.0 GPa

Show Material materials with Shear modulus of 25.9 - 26.0 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

24.0 - 25.9 GPa

Show Material materials with Shear modulus of 24.0 - 25.9 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

25.9 GPa

Show Material materials with Shear modulus of 25.9 GPa

H112

EN 573-3

Profile, Rod, Flat, Tube

Unlock all property charts

Tensile strength

20.0 °C

75.0 MPa

Show Material materials with Tensile strength of 75.0 MPa

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

85.0 MPa

Show Material materials with Tensile strength of 85.0 MPa

H112

EN 573-3

Flat

20.0 °C

80.0 MPa

Show Material materials with Tensile strength of 80.0 MPa

H112

EN 573-3

Flat

85.0 MPa

Show Material materials with Tensile strength of 85.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

80.0 MPa

Show Material materials with Tensile strength of 80.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

75.0 MPa

Show Material materials with Tensile strength of 75.0 MPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

85.0 MPa

Show Material materials with Tensile strength of 85.0 MPa

H112

EN 573-3

Flat

Transverse

20.0 °C

80.0 MPa

Show Material materials with Tensile strength of 80.0 MPa

H112

EN 573-3

Flat

Transverse

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

300 °C, 20 °C

2.5399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

200 °C, 20 °C

2.4399999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C, 20 °C, 100.0 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20 °C, -50 °C, -50.0 °C

2.17e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

200.0 °C

2.44e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K

H112

EN 573-3

Profile, Rod, Flat, Tube

300.0 °C

2.54e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K

H112

EN 573-3

Profile, Rod, Flat, Tube

Unlock all property charts

Melting point

644.0 - 657.0 °C

Show Material materials with Melting point of 644.0 - 657.0 °C

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

20.0 °C

898.0 J/(kg·K)

Show Material materials with Specific heat capacity of 898.0 J/(kg·K)

H112

EN 573-3

Profile, Rod, Flat, Tube

Thermal conductivity

20.0 °C

205.0 - 210.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 210.0 W/(m·K)

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat

20.0 °C

210.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 210.0 - 225.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

205.0 - 225.0 W/(m·K)

Show Material materials with Thermal conductivity of 205.0 - 225.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Flat, Tube

20.0 °C

225.0 W/(m·K)

Show Material materials with Thermal conductivity of 225.0 W/(m·K)

H112

EN 573-3

Profile, Rod, Flat, Tube

Unlock all property charts

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

34400000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34400000.0 - 35500000.0 S/m

H112

EN 573-3

Profile, Rod, Flat, Tube

33000000.0 - 34000000.0 S/m

Show Material materials with Electrical conductivity of 33000000.0 - 34000000.0 S/m

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Electrical resistivity

20.0 °C

2.95e-08 Ω·m

Show Material materials with Electrical resistivity of 2.95e-08 Ω·m

H112

EN 573-3

Profile, Rod, Flat, Tube

2.94e-08 - 3.03e-08 Ω·m

Show Material materials with Electrical resistivity of 2.94e-08 - 3.03e-08 Ω·m

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.0 %

Show Material materials with Aluminium of 99.0 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Manganese

0.05 %

Show Material materials with Manganese of 0.05 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Titanium

0.05 %

Show Material materials with Titanium of 0.05 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: sufficient, weathering: acceptable

Workability

Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12)