General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 0.35 % Show Supplier Material materials with Absorción de agua of 0.35 % | dry | ISO 62 | at 23°C after 24h |
4.7 % Show Supplier Material materials with Absorción de agua of 4.7 % | dry | Sim. to ISO 62 | ||
Densidad | 1.55 g/cm³ Show Supplier Material materials with Densidad of 1.55 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 2.1 % Show Supplier Material materials with Elongación of 2.1 % | conditioned | ISO 527-1/-2 |
-40 °C | 2.2 % Show Supplier Material materials with Elongación of 2.2 % | dry | ISO 527-1/-2 | |
2.2 % Show Supplier Material materials with Elongación of 2.2 % | conditioned | ISO 527-1/-2 | ||
2.3 % Show Supplier Material materials with Elongación of 2.3 % | dry | ISO 527-1/-2 | ||
40 °C | 2.1 % Show Supplier Material materials with Elongación of 2.1 % | conditioned | ISO 527-1/-2 | |
40 °C | 2.2 % Show Supplier Material materials with Elongación of 2.2 % | dry | ISO 527-1/-2 | |
80 °C | 2.5 % Show Supplier Material materials with Elongación of 2.5 % | dry | ISO 527-1/-2 | |
80 °C | 4.5 % Show Supplier Material materials with Elongación of 4.5 % | conditioned | ISO 527-1/-2 | |
100 °C | 3 % Show Supplier Material materials with Elongación of 3 % | dry | ISO 527-1/-2 | |
100 °C | 5 % Show Supplier Material materials with Elongación of 5 % | conditioned | ISO 527-1/-2 | |
120 °C | 5.1 % Show Supplier Material materials with Elongación of 5.1 % | dry | ISO 527-1/-2 | |
120 °C | 6 % Show Supplier Material materials with Elongación of 6 % | conditioned | ISO 527-1/-2 | |
150 °C | 6.9 % Show Supplier Material materials with Elongación of 6.9 % | dry | ISO 527-1/-2 | |
160 °C | 7 % Show Supplier Material materials with Elongación of 7 % | dry | ISO 527-1/-2 | |
180 °C | 7 % Show Supplier Material materials with Elongación of 7 % | dry | ISO 527-1/-2 | |
200 °C | 7 % Show Supplier Material materials with Elongación of 7 % | dry | ISO 527-1/-2 | |
210 °C | 0.007 % Show Supplier Material materials with Elongación of 0.007 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 290 MPa Show Supplier Material materials with Flexural yield strength of 290 MPa | conditioned | ISO 178 | |
350 MPa Show Supplier Material materials with Flexural yield strength of 350 MPa | dry | ISO 178 | ||
120 °C | 200 MPa Show Supplier Material materials with Flexural yield strength of 200 MPa | dry | ISO 178 | |
160 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |
180 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
200 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
210 °C | 95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | |
Módulo de flexión | 14 GPa Show Supplier Material materials with Módulo de flexión of 14 GPa | dry | ISO 178 | |
14.5 GPa Show Supplier Material materials with Módulo de flexión of 14.5 GPa | conditioned | ISO 178 | ||
120 °C | 9.8 GPa Show Supplier Material materials with Módulo de flexión of 9.8 GPa | dry | ISO 178 | |
160 °C | 6 GPa Show Supplier Material materials with Módulo de flexión of 6 GPa | dry | ISO 178 | |
180 °C | 5.4 GPa Show Supplier Material materials with Módulo de flexión of 5.4 GPa | dry | ISO 178 | |
200 °C | 5 GPa Show Supplier Material materials with Módulo de flexión of 5 GPa | dry | ISO 178 | |
210 °C | 4.9 GPa Show Supplier Material materials with Módulo de flexión of 4.9 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 14.8 GPa Show Supplier Material materials with Módulo elástico of 14.8 GPa | dry | ISO 527-1/-2 |
-40 °C | 15 GPa Show Supplier Material materials with Módulo elástico of 15 GPa | conditioned | ISO 527-1/-2 | |
14.5 GPa Show Supplier Material materials with Módulo elástico of 14.5 GPa | dry | ISO 527-1/-2 | ||
14.8 GPa Show Supplier Material materials with Módulo elástico of 14.8 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 14 GPa Show Supplier Material materials with Módulo elástico of 14 GPa | conditioned | ISO 527-1/-2 | |
40 °C | 14.2 GPa Show Supplier Material materials with Módulo elástico of 14.2 GPa | dry | ISO 527-1/-2 | |
80 °C | 8.8 GPa Show Supplier Material materials with Módulo elástico of 8.8 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 13.5 GPa Show Supplier Material materials with Módulo elástico of 13.5 GPa | dry | ISO 527-1/-2 | |
100 °C | 7 GPa Show Supplier Material materials with Módulo elástico of 7 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 12.8 GPa Show Supplier Material materials with Módulo elástico of 12.8 GPa | dry | ISO 527-1/-2 | |
120 °C | 6.3 GPa Show Supplier Material materials with Módulo elástico of 6.3 GPa | conditioned | ISO 527-1/-2 | |
120 °C | 9.5 GPa Show Supplier Material materials with Módulo elástico of 9.5 GPa | dry | ISO 527-1/-2 | |
150 °C | 6.7 GPa Show Supplier Material materials with Módulo elástico of 6.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 6.3 GPa Show Supplier Material materials with Módulo elástico of 6.3 GPa | dry | ISO 527-1/-2 | |
180 °C | 5.5 GPa Show Supplier Material materials with Módulo elástico of 5.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 5.3 GPa Show Supplier Material materials with Módulo elástico of 5.3 GPa | dry | ISO 527-1/-2 | |
210 °C | 5 GPa Show Supplier Material materials with Módulo elástico of 5 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 250 MPa Show Supplier Material materials with Resistencia a la tracción of 250 MPa | dry, conditioned | ISO 527-1/-2 |
210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | conditioned | ISO 527-1/-2 | ||
230 MPa Show Supplier Material materials with Resistencia a la tracción of 230 MPa | dry | ISO 527-1/-2 | ||
40 °C | 190 MPa Show Supplier Material materials with Resistencia a la tracción of 190 MPa | conditioned | ISO 527-1/-2 | |
40 °C | 220 MPa Show Supplier Material materials with Resistencia a la tracción of 220 MPa | dry | ISO 527-1/-2 | |
80 °C | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 200 MPa Show Supplier Material materials with Resistencia a la tracción of 200 MPa | dry | ISO 527-1/-2 | |
100 °C | 100 MPa Show Supplier Material materials with Resistencia a la tracción of 100 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 170 MPa Show Supplier Material materials with Resistencia a la tracción of 170 MPa | dry | ISO 527-1/-2 | |
120 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | conditioned | ISO 527-1/-2 | |
120 °C | 140 MPa Show Supplier Material materials with Resistencia a la tracción of 140 MPa | dry | ISO 527-1/-2 | |
150 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | dry | ISO 527-1/-2 | |
160 °C | 95 MPa Show Supplier Material materials with Resistencia a la tracción of 95 MPa | dry | ISO 527-1/-2 | |
180 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
200 °C | 78 MPa Show Supplier Material materials with Resistencia a la tracción of 78 MPa | dry | ISO 527-1/-2 | |
210 °C | 73 MPa Show Supplier Material materials with Resistencia a la tracción of 73 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 8 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 10 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 10 kJ/m² | dry | ISO 179/1eA | |
23 °C | 9 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 55.0 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 55.0 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | dry | ISO 179/1eU | |
23 °C | 60 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 60 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 70 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 70 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 3e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3e-07 1/K | dry | ASTM D696 | Parallel | |
3.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 3.5e-07 1/K | dry | ASTM D696 | Normal | ||
Temperatura de flexión bajo carga | 305 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 305 °C | dry | ISO 75-1/-2 | 2 MPa | |
317 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 317 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Temperatura de fusión | 325 °C Show Supplier Material materials with Temperatura de fusión of 325 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Temperatura de transición del vidrio | 125 °C Show Supplier Material materials with Temperatura de transición del vidrio of 125 °C | dry | ISO 11357-1/-2 | 10°C/min | |
130 °C Show Supplier Material materials with Temperatura de transición del vidrio of 130 °C | dry | ASTM D5026/D7028 | DMTA (tan d) |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4.6 [-] Show Supplier Material materials with Constante dieléctrica of 4.6 [-] | dry | IEC 62631-2-1 | 1MHz |
4.8 [-] Show Supplier Material materials with Constante dieléctrica of 4.8 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
4.9 [-] Show Supplier Material materials with Constante dieléctrica of 4.9 [-] | dry | IEC 62631-2-1 | 100Hz | |
5.7 [-] Show Supplier Material materials with Constante dieléctrica of 5.7 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 57 [-] Show Supplier Material materials with Factor de disipación of 57 [-] | dry | IEC 62631-2-1 | 100Hz |
180 [-] Show Supplier Material materials with Factor de disipación of 180 [-] | dry | IEC 62631-2-1 | 1MHz | |
270 [-] Show Supplier Material materials with Factor de disipación of 270 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
290 [-] Show Supplier Material materials with Factor de disipación of 290 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Crankshaft Covers | |
Fillers | 40% Glass Fiber |