General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Absorción de agua | 2.65 % Show Supplier Material materials with Absorción de agua of 2.65 % | dry | ISO 62 | at 23°C after 24h |
9.5 % Show Supplier Material materials with Absorción de agua of 9.5 % | dry | Sim. to ISO 62 | ||
Densidad | 1.41 g/cm³ Show Supplier Material materials with Densidad of 1.41 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.6 % Show Supplier Material materials with Moisture absorption of 2.6 % | dry | Sim. to ISO 62 |
Mecánica
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elongación | -40 °C | 3.5 % Show Supplier Material materials with Elongación of 3.5 % | dry | ISO 527-1/-2 |
3.7 % Show Supplier Material materials with Elongación of 3.7 % | dry | ISO 527-1/-2 | ||
6 % Show Supplier Material materials with Elongación of 6 % | conditioned | ISO 527-1/-2 | ||
120 °C | 7.5 % Show Supplier Material materials with Elongación of 7.5 % | dry | ISO 527-1/-2 | |
140 °C | 8 % Show Supplier Material materials with Elongación of 8 % | dry | ISO 527-1/-2 | |
150 °C | 8 % Show Supplier Material materials with Elongación of 8 % | dry | ISO 527-1/-2 | |
160 °C | 8 % Show Supplier Material materials with Elongación of 8 % | dry | ISO 527-1/-2 | |
180 °C | 8 % Show Supplier Material materials with Elongación of 8 % | dry | ISO 527-1/-2 | |
200 °C | 8 % Show Supplier Material materials with Elongación of 8 % | dry | ISO 527-1/-2 | |
210 °C | 0.008 % Show Supplier Material materials with Elongación of 0.008 % | dry | ISO 527-1/-2 | |
Flexural yield strength | 180 MPa Show Supplier Material materials with Flexural yield strength of 180 MPa | conditioned | ISO 178 | |
300 MPa Show Supplier Material materials with Flexural yield strength of 300 MPa | dry | ISO 178 | ||
120 °C | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | dry | ISO 178 | |
160 °C | 130 MPa Show Supplier Material materials with Flexural yield strength of 130 MPa | dry | ISO 178 | |
180 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
200 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |
210 °C | 105 MPa Show Supplier Material materials with Flexural yield strength of 105 MPa | dry | ISO 178 | |
Módulo de flexión | 5.5 GPa Show Supplier Material materials with Módulo de flexión of 5.5 GPa | conditioned | ISO 178 | |
9.5 GPa Show Supplier Material materials with Módulo de flexión of 9.5 GPa | dry | ISO 178 | ||
120 °C | 5.1 GPa Show Supplier Material materials with Módulo de flexión of 5.1 GPa | dry | ISO 178 | |
160 °C | 4.9 GPa Show Supplier Material materials with Módulo de flexión of 4.9 GPa | dry | ISO 178 | |
180 °C | 4.5 GPa Show Supplier Material materials with Módulo de flexión of 4.5 GPa | dry | ISO 178 | |
200 °C | 4.4 GPa Show Supplier Material materials with Módulo de flexión of 4.4 GPa | dry | ISO 178 | |
210 °C | 4.4 GPa Show Supplier Material materials with Módulo de flexión of 4.4 GPa | dry | ISO 178 | |
Módulo elástico | -40 °C | 10.2 GPa Show Supplier Material materials with Módulo elástico of 10.2 GPa | dry | ISO 527-1/-2 |
6 GPa Show Supplier Material materials with Módulo elástico of 6 GPa | conditioned | ISO 527-1/-2 | ||
10 GPa Show Supplier Material materials with Módulo elástico of 10 GPa | dry | ISO 527-1/-2 | ||
40 °C | 9.5 GPa Show Supplier Material materials with Módulo elástico of 9.5 GPa | dry | ISO 527-1/-2 | |
100 °C | 5.5 GPa Show Supplier Material materials with Módulo elástico of 5.5 GPa | dry | ISO 527-1/-2 | |
120 °C | 5.3 GPa Show Supplier Material materials with Módulo elástico of 5.3 GPa | dry | ISO 527-1/-2 | |
140 °C | 5.1 GPa Show Supplier Material materials with Módulo elástico of 5.1 GPa | dry | ISO 527-1/-2 | |
150 °C | 5 GPa Show Supplier Material materials with Módulo elástico of 5 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.8 GPa Show Supplier Material materials with Módulo elástico of 4.8 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.5 GPa Show Supplier Material materials with Módulo elástico of 4.5 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.3 GPa Show Supplier Material materials with Módulo elástico of 4.3 GPa | dry | ISO 527-1/-2 | |
210 °C | 4.2 GPa Show Supplier Material materials with Módulo elástico of 4.2 GPa | dry | ISO 527-1/-2 | |
Resistencia a la tracción | -40 °C | 250 MPa Show Supplier Material materials with Resistencia a la tracción of 250 MPa | dry | ISO 527-1/-2 |
115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | conditioned | ISO 527-1/-2 | ||
210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | dry | ISO 527-1/-2 | ||
100 °C | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | dry | ISO 527-1/-2 | |
120 °C | 115 MPa Show Supplier Material materials with Resistencia a la tracción of 115 MPa | dry | ISO 527-1/-2 | |
140 °C | 110 MPa Show Supplier Material materials with Resistencia a la tracción of 110 MPa | dry | ISO 527-1/-2 | |
150 °C | 105 MPa Show Supplier Material materials with Resistencia a la tracción of 105 MPa | dry | ISO 527-1/-2 | |
160 °C | 100 MPa Show Supplier Material materials with Resistencia a la tracción of 100 MPa | dry | ISO 527-1/-2 | |
180 °C | 95 MPa Show Supplier Material materials with Resistencia a la tracción of 95 MPa | dry | ISO 527-1/-2 | |
200 °C | 90 MPa Show Supplier Material materials with Resistencia a la tracción of 90 MPa | dry | ISO 527-1/-2 | |
210 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | dry | ISO 527-1/-2 | |
Resistencia al choque, ensayo Charpy entallado | -30 °C | 11 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 11 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 12 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | dry | ISO 179/1eA | |
23 °C | 21 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 21 kJ/m² | conditioned | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30 °C | 65 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 65 kJ/m² | dry | ISO 179/1eU |
-30 °C | 75 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 75 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 80 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 100 kJ/m² | conditioned | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coeficiente de dilatación térmica | 2.5e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6e-07 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Difusividad térmica | 1.1e-07 mm²/s Show Supplier Material materials with Difusividad térmica of 1.1e-07 mm²/s | dry | - | |||
Glow Wire Flammability Index | 650 °C Show Supplier Material materials with Glow Wire Flammability Index of 650 °C | dry | IEC 60695-2-12 | 0.75 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | |||
Glow Wire Ignition Temperature | 700 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 700 °C | dry | IEC 60695-2-13 | 0.75 mm | ||
725 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 725 °C | dry | IEC 60695-2-13 | 3 mm | |||
Inflamabilidad | HB | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm | ||
Temperatura de flexión bajo carga | 290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Temperatura de flexión bajo carga of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Temperatura de fusión | 295 °C Show Supplier Material materials with Temperatura de fusión of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Temperatura de reblandecimiento Vicat | 290 °C Show Supplier Material materials with Temperatura de reblandecimiento Vicat of 290 °C | dry | ISO 306 | 50°C/h 50N | ||
Temperatura de transición del vidrio | 75 °C Show Supplier Material materials with Temperatura de transición del vidrio of 75 °C | dry | ISO 11357-1/-2 | 10°C/min |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Constante dieléctrica | 4 [-] Show Supplier Material materials with Constante dieléctrica of 4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.3 [-] Show Supplier Material materials with Constante dieléctrica of 4.3 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.7 [-] Show Supplier Material materials with Constante dieléctrica of 4.7 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
16 [-] Show Supplier Material materials with Constante dieléctrica of 16 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Factor de disipación | 70 [-] Show Supplier Material materials with Factor de disipación of 70 [-] | dry | IEC 62631-2-1 | 100Hz |
200 [-] Show Supplier Material materials with Factor de disipación of 200 [-] | dry | IEC 62631-2-1 | 1MHz | |
1000 [-] Show Supplier Material materials with Factor de disipación of 1000 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
6000 [-] Show Supplier Material materials with Factor de disipación of 6000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Rigidez dieléctrica | 20 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 20 kV/mm | conditioned | IEC 60243-1 | |
30 kV/mm Show Supplier Material materials with Rigidez dieléctrica of 30 kV/mm | dry | IEC 60243-1 | ||
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+07 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+07 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 | ||
Índice de seguimiento comparativo | 300 V Show Supplier Material materials with Índice de seguimiento comparativo of 300 V | dry | IEC 60112 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Contracción | 0.5 % Show Supplier Material materials with Contracción of 0.5 % | dry | Sim. to ISO 294-4 | Parallel |
1.3 % Show Supplier Material materials with Contracción of 1.3 % | dry | Sim. to ISO 294-4 | Normal | |
Density of melt | 1210 g/cm³ Show Supplier Material materials with Density of melt of 1210 g/cm³ | dry | - | |
Specific heat capacity melt | 2200 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2200 J/(kg·K) | dry | - | |
Spiral flow length | 100 | dry | - | 1.0 mm 800 bar |
110 | dry | - | 1.0 mm 900 bar | |
120 | dry | - | 1.0 mm 1000 bar | |
33 | dry | - | 0.5mm 1200 bar | |
44 | dry | - | 0.5mm 1600 bar | |
76 | dry | - | 0.5mm 2000 bar | |
Thermal conductivity of melt | 0.296 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.296 W/(m·K) | dry | - | |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Application areas | Automotive Bearing Cages, Wheel Speed Sensors, Endlaminates (electrical components), Electronic throttle control actuators, Exhaust gas recirculation actuators, Turbo actuators, Coolant valve actuators | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |