Description

EN AW-5657 is a non-heat treatable alloy that offers users workability and medium strength. Due to the addition of magnesium to the alloy, EN AW-5657 has enhanced corrosion resistance. EN AW-5657 can be welded with most convention methods including resistance welding, arc, and gas torch. This alloy can be both hot and cold formed as well as brazed, however it only offers fair machinability and getting the perfect finish takes extra work.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H22

EN 573-3, EN 485

Strip, Sheet, Plate

2.69 g/cm³

Show Material materials with Density of 2.69 g/cm³

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.3 mm

Show Material materials with Thickness of 0.3 mm

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.3 mm

Coil, Sheet, Strip

1.2 mm

Show Material materials with Thickness of 1.2 mm

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

1.2 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H22

EN 573-3, EN 485

Strip, Sheet, Plate

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Tensile strength

120.0 - 160.0 MPa

Show Material materials with Tensile strength of 120.0 - 160.0 MPa

H22

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Coil, Sheet, Strip

20.0 °C

110.0 - 160.0 MPa

Show Material materials with Tensile strength of 110.0 - 160.0 MPa

H22

EN 573-3

Flat

Transverse

Yield strength

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

H22

EN 573-3, EN 485

Strip, Sheet, Plate

RP02

80 MPa

Show Material materials with Yield strength of 80 MPa

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20.0 °C

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

H22

EN 573-3

Flat

RP02 Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H22

EN 573-3, EN 485

Strip, Sheet, Plate

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H22

EN 573-3, EN 485

Strip, Sheet, Plate

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

635.0 - 655.0 °C

Show Material materials with Melting point of 635.0 - 655.0 °C

H22

EN 573-3, EN 485

Strip, Sheet, Plate

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

138 W/(m·K)

Show Material materials with Thermal conductivity of 138 W/(m·K)

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

205 W/(m·K)

Show Material materials with Thermal conductivity of 205 W/(m·K)

H22

EN 573-3, EN 485

Strip, Sheet, Plate

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

31000000.0 S/m

Show Material materials with Electrical conductivity of 31000000.0 S/m

H22

EN 573-3, EN 485

Strip, Sheet, Plate

Electrical resistivity

3.23e-08 Ω·m

Show Material materials with Electrical resistivity of 3.23e-08 Ω·m

H22

EN 573-3, EN 485

Strip, Sheet, Plate

4.9e-08 Ω·m

Show Material materials with Electrical resistivity of 4.9e-08 Ω·m

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

0.1 %

Show Material materials with Copper of 0.1 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Gallium

0.03 %

Show Material materials with Gallium of 0.03 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

Iron

0.1 %

Show Material materials with Iron of 0.1 %

H22

EN 573-3

Flat

0.10 %

Show Material materials with Iron of 0.10 %

H22

EN 573-3, EN 485

Strip, Sheet, Plate

0.1 %

Show Material materials with Iron of 0.1 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Magnesium

0.6 - 1.0 %

Show Material materials with Magnesium of 0.6 - 1.0 %

H22

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Coil, Sheet, Strip

Manganese

0.03 %

Show Material materials with Manganese of 0.03 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

0.03 %

Show Material materials with Manganese of 0.03 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Other

0.05 %

Show Material materials with Other of 0.05 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Silicon

0.08 %

Show Material materials with Silicon of 0.08 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

0.08 %

Show Material materials with Silicon of 0.08 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Vanadium

0.05 %

Show Material materials with Vanadium of 0.05 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

H22

EN 573-3, EN 485

Flat, Strip, Sheet, Plate

0.05 %

Show Material materials with Zinc of 0.05 %

H22

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

Excellent

Application areas

Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels; Anodizing quality; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim, Window frame, Marque badges

Corrosion properties

Excellent

General machinability

Good

Welding

Good

Workability

Good