General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | O | EN 573-3, EN 485, EN 754, EN 755 | |||
Bending angle 180° | 0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Bending angle 90° | 1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | O | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | O | EN 573-3, EN 485 | ||||
2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | O | EN 573-3, EN 485 | ||||
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | O | EN 573-3, EN 485 | ||||
Elastic modulus | 73.0 GPa Show Material materials with Elastic modulus of 73.0 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 72.0 GPa Show Material materials with Elastic modulus of 72.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Elongation | 10.0 % Show Material materials with Elongation of 10.0 % | O | EN 573-3, EN 754, EN 755 | A50 | ||
10.0 % Show Material materials with Elongation of 10.0 % | O | EN 573-3, EN 485 | A100 | |||
12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3, EN 485 | A50 | |||
12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3, EN 754, EN 755 | A100 | |||
13.0 % Show Material materials with Elongation of 13.0 % | O | EN 573-3, EN 485 | A50 | |||
16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Hardness, Brinell | 55.0 [-] Show Material materials with Hardness, Brinell of 55.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 55.0 [-] Show Material materials with Hardness, Brinell of 55.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 27.4 GPa Show Material materials with Shear modulus of 27.4 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | |||
Tensile strength | 220.0 Show Material materials with Tensile strength of 220.0 | O | EN 573-3, EN 485 | |||
240.0 Show Material materials with Tensile strength of 240.0 | O | EN 573-3, EN 754 | ||||
250.0 Show Material materials with Tensile strength of 250.0 | O | EN 573-3, EN 755 | ||||
20.0 °C | 220.0 Show Material materials with Tensile strength of 220.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.1e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | |||
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
20 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
100 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | |||
200 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
300 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet | ||
Melting point | 505.0 - 635.0 °C Show Material materials with Melting point of 505.0 - 635.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | |||
510.0 - 640.0 °C Show Material materials with Melting point of 510.0 - 640.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | ||||
Specific heat capacity | 816.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Thermal conductivity | 134.0 - 193.0 W/(m·K) Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K) | O | EN 573-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 200.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 21000000.0 - 24000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 24000000.0 S/m | O | EN 573-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet | |
Electrical resistivity | 3.45e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 | ||
4.17e-08 - 4.76e-08 Ω·m Show Material materials with Electrical resistivity of 4.17e-08 - 4.76e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Copper | 3.9 - 5.0 % Show Material materials with Copper of 3.9 - 5.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet |
0.70 % Show Material materials with Iron of 0.70 % | O | EN 573-3, EN 485, EN 754, EN 755 | ||
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Manganese | 0.4 - 1.2 % Show Material materials with Manganese of 0.4 - 1.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Silicon | 0.5 - 1.2 % Show Material materials with Silicon of 0.5 - 1.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754, EN 755 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |