General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Mechanical
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | F | EN 573-3, EN 14121 | Strip, Sheet, Plate | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Shear modulus | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |||
Tensile strength | 65.0 MPa Show Material materials with Tensile strength of 65.0 MPa | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | F | EN 573-3, EN 14121 | Strip, Sheet, Plate | |
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | F | EN 573-3, EN 14121 | Strip, Sheet, Plate | ||
Melting point | 658.0 °C Show Material materials with Melting point of 658.0 °C | F | EN 573-3, EN 14121 | Strip, Sheet, Plate | ||
Specific heat capacity | 900.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Thermal conductivity | 230 W/(m·K) Show Material materials with Thermal conductivity of 230 W/(m·K) | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Electrical
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Electrical conductivity | 34500000.0 - 35500000.0 S/m Show Material materials with Electrical conductivity of 34500000.0 - 35500000.0 S/m | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Electrical resistivity | 2.82e-08 - 2.9e-08 Ω·m Show Material materials with Electrical resistivity of 2.82e-08 - 2.9e-08 Ω·m | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Copper | 0.02 % Show Material materials with Copper of 0.02 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Iron | 0.40 % Show Material materials with Iron of 0.40 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | F | EN 573-3, EN 14121 | Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good, general: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |