Soft glass, free from sodium, of high lead content, lower sealing temperature than glass 8531.
See where Lead Glass SCHOTT 8532 falls on the material property chart for Density against Elastic modulus in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.
Density
ρ4.46 g/cm³ at 20 °C
Annealing temperature
Tanneal430 °C
Viscosity 10¹³ dPa.s (ISO 7884-4)
Coefficient of thermal expansion
α8.7E-6 1/K at 20 °C
mean value for 20-300 °C - ISO 7991
Glass transition temperature
Tg435 °C
ISO 7884-8
Softening temperature
Tsoftening560 °C
Viscosity 10⁷·⁶ dPa.s (ISO 7884-3)
Specific electrical resistance temperature
Tk440 °C
For ρ = 10⁸ Ω·cm
Thermal conductivity
λ0.7 W/(m·K) at 90 °C
Working temperature
Tworking760 °C
Viscosity 10⁴ dPa.s (ISO 7884-2)
Dielectric constant, 1MHz
εr,1MHz10.2 [-] at 20 °C
Electrical resistivity
ρel1.00E+9 Ω·m at 250 °C
Loss tangent, 1MHz
tanδ1,MHz9E-4 [-] at 20 °C
Refractive index
nd1.72 [-]
at λ=587.6 nm
Stress optical coefficient
k1.7E-6 mm²/N
DIN 52314
Application areas
Encapsulation of semiconductor components at low temperature (Microdiodes), Electronics, Sensors
Corrosion properties
Hydrolytic resistance Class HGB1 (ISO 719) - Acid resistance Class S4 (DIN 12116) - Alkali resistance Class A3 (ISO695)
This material data has been provided by Schott Glass Tubing.