Description

Glass tubes for sealing to kovar. High transmittance and chemically highly resistance

This material data has been provided by Schott Glass Tubing.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

2.34 g/cm³

Show Supplier Material materials with Density of 2.34 g/cm³

Mechanical

PropertyValue

Elastic modulus

73 GPa

Show Supplier Material materials with Elastic modulus of 73 GPa

Thermal

PropertyValueTesting StandardComment

Annealing temperature

570.0 °C

Show Supplier Material materials with Annealing temperature of 570.0 °C

ISO 7884-4

Viscosity 10¹³ dPa·s

Coefficient of thermal expansion

5.5e-06 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 5.5e-06 1/K

ISO 7991

mean value for 20-300 °C

Glass transition temperature

565 °C

Show Supplier Material materials with Glass transition temperature of 565 °C

ISO 7884-8

Softening temperature

790.0 °C

Show Supplier Material materials with Softening temperature of 790.0 °C

ISO 7884-3

Viscosity 10⁷·⁶ dPa·s

Specific electrical resistance temperature

191.0 °C

Show Supplier Material materials with Specific electrical resistance temperature of 191.0 °C

For ρ=10⁸ Ω·cm

Working temperature

1175.0 °C

Show Supplier Material materials with Working temperature of 1175.0 °C

ISO 7884-2

Viscosity 10⁴ dPa·s

Electrical

PropertyTemperatureValueFrequency

Dielectric constant

5.9 [-]

Show Supplier Material materials with Dielectric constant of 5.9 [-]

1MHz

Electrical resistivity

250 °C

100000 Ω·m

Show Supplier Material materials with Electrical resistivity of 100000 Ω·m

350 °C

5012 Ω·m

Show Supplier Material materials with Electrical resistivity of 5012 Ω·m

Loss tangent

0.0143 [-]

Show Supplier Material materials with Loss tangent of 0.0143 [-]

1MHz

Optical

PropertyValueTesting StandardComment

Refractive index

1.5 [-]

Show Supplier Material materials with Refractive index of 1.5 [-]

at λ=587.6 nm

Stress optical coefficient

3.3e-06 mm²/N

Show Supplier Material materials with Stress optical coefficient of 3.3e-06 mm²/N

DIN 52314

Chemical properties

Property

Other

0.01 %

max., Lead, Cadmium, Mercury and Hexavalent Chromium

Technological properties

Property
Application areas

Renewable energies (Receiver), Fibre Optics

Corrosion properties

Hydrolytic resistance Class HGB1 (ISO 719) - Acid resistance Class S1 (DIN 12116) - Alkali resistance Class A2 (ISO695)