DIN 1725-1 Grade 3.4365 T62

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlZnMgCu1,5 as a Cu-alloyed AlZnMg-alloy achieves highest strength values due to its composition. Strength grade F 55 is achievable by artificial aging. Heat-treatment for hardening: solution annealing: 470 to 480 °C quenching in water artificial aging: 12 to 24 h at 115 to 125 °C 4 to 6 h at 165 to 180 °C The artificial aging represents a two-step aging. Natural aging is unusual. The alloy has a favorable machinability and it is on certain conditions weldable. When welding appears a heat-affected zone of lower strength therefore welding should be avoided. A favorable corrosion resistance can only be warranted for an appropriate surface protection coat. Corrosion resistance can be considerably enhanced by artificial aging. In order to tap the full strength values, without having any negative effect of the lower corrosion resistance, the sheets of this alloy are cladded by rolling with e.g. AlZn1. Therby the application area expands considerably. Furthermore the alloy has a favorable machinability. Application: In machine engineering (incl. mold making) for appliances and tools. Predominantly as anchor, head and punch unit holder plates as well as for guide plates. In mold making esp. in plastics processing for blow, foam and injection forms, carrying constructions for woodworking tools, for machine benchings, turned parts (hydraulics/pneumatics), in vehicle manufacturing for bumper, safety parts. In aircraft construction as connecting elements (screws), in military engineering for bending and forming technics (as wire: springs, screens, hooks etc.).

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

Mechanical

PropertyTemperatureValueComment

Bulk Modulus

20.0 °C

72.5 GPa

Show Material materials with Bulk Modulus of 72.5 GPa

Elastic modulus

20.0 °C

71 GPa

Show Material materials with Elastic modulus of 71 GPa

Elongation

20.0 °C

6 - 8 %

Show Material materials with Elongation of 6 - 8 %

Elongation, transverse

20.0 °C

8 %

Show Material materials with Elongation, transverse of 8 %

Hardness, Brinell

20.0 °C

140 [-]

Show Material materials with Hardness, Brinell of 140 [-]

Hardness, Brinell, trans

20.0 °C

140 [-]

Show Material materials with Hardness, Brinell, trans of 140 [-]

Plane-Strain Fracture Toughnes

23.0 °C

22 - 35 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

23.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

23.0 °C

26.4 - 27.1 GPa

Show Material materials with Shear modulus of 26.4 - 27.1 GPa

Typical for Wrought 7000 Series Aluminium

Tensile strength

20.0 °C

520 - 540 MPa

Show Material materials with Tensile strength of 520 - 540 MPa

Tensile strength, transverse

20.0 °C

530 MPa

Show Material materials with Tensile strength, transverse of 530 MPa

Yield strength Rp0.2

20.0 °C

470 - 490 MPa

Show Material materials with Yield strength Rp0.2 of 470 - 490 MPa

Yield strength Rp0.2, transverse

20.0 °C

450 MPa

Show Material materials with Yield strength Rp0.2, transverse of 450 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.1E-5 - 2.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.1E-5 - 2.4E-5 1/K

Typical for Wrought 7000 Series Aluminium

Melting point

465 - 655 °C

Show Material materials with Melting point of 465 - 655 °C

Typical for Wrought 7000 Series Aluminium

Specific heat capacity

23.0 °C

795 - 1050 J/(kg·K)

Show Material materials with Specific heat capacity of 795 - 1050 J/(kg·K)

Typical for Wrought 7000 Series Aluminium

Thermal conductivity

23.0 °C

121 - 170 W/(m·K)

Show Material materials with Thermal conductivity of 121 - 170 W/(m·K)

Typical for Wrought 7000 Series Aluminium

Electrical

PropertyTemperatureValueComment

Electrical conductivity

23.0 °C

1.80E+7 - 3.40E+7 S/m

Show Material materials with Electrical conductivity of 1.80E+7 - 3.40E+7 S/m

Typical for Wrought 7000 Series Aluminium

Electrical resistivity

23.0 °C

2.9E-8 - 5.6E-8 Ω·m

Show Material materials with Electrical resistivity of 2.9E-8 - 5.6E-8 Ω·m

Typical for Wrought 7000 Series Aluminium

Chemical properties

PropertyValue

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

Copper

1.2 - 2 %

Show Material materials with Copper of 1.2 - 2 %

Iron

0.5 %

Show Material materials with Iron of 0.5 %

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

Technological properties

Property
Brazing

Excellent