Molybdenum Annealed, Electropolished Wire

Want to keep this datasheet? Save it now in your required format

Description

With its unique mechanical and chemical properties, molybdenum is an outstanding material that can meet the most exacting requirements. Because molybdenum possesses a very high melting point, a low coefficient of thermal expansion and a high level of thermal conductivity, it is used in many different industries. Molybdenum is a genuine all-rounder.

This material data has been provided by Plansee.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValue

Density

23.0 °C

10.2 g/cm³

Show Supplier Material materials with Density of 10.2 g/cm³

Neutron capture cross-section

23.0 °C

0 m²

Show Supplier Material materials with Neutron capture cross-section of 0 m²

Dimension

PropertyValue

Diameter

0.5 - 1 mm

Show Supplier Material materials with Diameter of 0.5 - 1 mm

Dimensions

Available diameters (mm): 0.5; 1

Mechanical

PropertyTemperatureValue

Elongation

23.0 °C

10 %

Show Supplier Material materials with Elongation of 10 %

Tensile strength

23.0 °C

750 - 1200 MPa

Show Supplier Material materials with Tensile strength of 750 - 1200 MPa

Thermal

PropertyValue

Melting point

2620 °C

Show Supplier Material materials with Melting point of 2620 °C

Electrical

PropertyTemperatureValue

Electron work function

23.0 °C

4.39 eV

Show Supplier Material materials with Electron work function of 4.39 eV

Acoustical

PropertyTemperatureValue

Sound speed, longitudinal

23.0 °C

6250 m/s

Show Supplier Material materials with Sound speed, longitudinal of 6250 m/s

Sound speed, transversal

23.0 °C

3350 m/s

Show Supplier Material materials with Sound speed, transversal of 3350 m/s

Chemical properties

PropertyValue

Aluminium

1E-4 %

Show Supplier Material materials with Aluminium of 1E-4 %

Cadmium

1E-4 %

Show Supplier Material materials with Cadmium of 1E-4 %

Carbon

1.3E-3 %

Show Supplier Material materials with Carbon of 1.3E-3 %

Chromium

3E-4 %

Show Supplier Material materials with Chromium of 3E-4 %

Copper

2E-4 %

Show Supplier Material materials with Copper of 2E-4 %

Iron

5E-4 %

Show Supplier Material materials with Iron of 5E-4 %

Molybdenum

99.97 %

Show Supplier Material materials with Molybdenum of 99.97 %

Nickel

1E-4 %

Show Supplier Material materials with Nickel of 1E-4 %

Nitrogen

5E-4 %

Show Supplier Material materials with Nitrogen of 5E-4 %

Oxygen

6E-4 %

Show Supplier Material materials with Oxygen of 6E-4 %

Potassium

6E-4 %

Show Supplier Material materials with Potassium of 6E-4 %

Silicon

2E-4 %

Show Supplier Material materials with Silicon of 2E-4 %

Tungsten

0.02 %

Show Supplier Material materials with Tungsten of 0.02 %

Technological properties

Property