RADILON A CP300K 333 BK

Alternative and trade names
PA66-T MD30, PA66-MD30
Want to keep this datasheet? Save it now in your required format

Description

PA66 30% mineral filled injection moulding grade. Heat stabilized. Black colour.

Suitable for parts requiring good dimensional stability, reduced shrinkage and low warpage.

This material data has been provided by Radici Group.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.35 g/cm³

Show Supplier Material materials with Density of 1.35 g/cm³

ISO 1183, DAM

Moisture absorption

23.0 °C

1.9 %

Show Supplier Material materials with Moisture absorption of 1.9 %

ISO 62, 50% RH, thickness tested (mm): 2

Water absorption

23.0 °C

6.1 %

Show Supplier Material materials with Water absorption of 6.1 %

ISO 62, thickness tested (mm): 2

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

4.8 GPa

Show Supplier Material materials with Elastic modulus of 4.8 GPa

ISO 527-2/1A, 1mm/min, DAM

Elongation

23.0 °C

6 %

Show Supplier Material materials with Elongation of 6 %

ISO 527-2/1A, 5mm/min, DAM

Flexural modulus

23.0 °C

4.9 GPa

Show Supplier Material materials with Flexural modulus of 4.9 GPa

ISO 178, 2mm/min, DAM

Flexural strength

23.0 °C

150 MPa

Show Supplier Material materials with Flexural strength of 150 MPa

ISO 178, 2mm/min, DAM

Impact strength, Charpy notched

23.0 °C

4 - 30 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 4 - 30 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-30.0 °C

40 kJ/m²

Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m²

ISO 179/1eU

23.0 °C

55 kJ/m²

Show Supplier Material materials with Impact strength, Charpy unnotched of 55 kJ/m²

ISO 179/1eU

Tensile strength

23.0 °C

85 MPa

Show Supplier Material materials with Tensile strength of 85 MPa

ISO 527-2/1A, 5mm/min, DAM

Thermal

PropertyValueComment

Heat deflection temperature, 0.45 MPa

215 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 215 °C

ISO 75/2Bf

Heat deflection temperature, 1.80 MPa

90 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 90 °C

ISO 75/2Af

Melting point

260 °C

Show Supplier Material materials with Melting point of 260 °C

ISO 11357-1/-3, 10°C/min

Vicat softening temperature

245 °C

Show Supplier Material materials with Vicat softening temperature of 245 °C

ISO 306, 50°C/h 50N

Flammability

Automotive Interior Flammability(mm/min): 0 ,method: ISO 3795 and thickness tested (mm): 3 | Class: HB ,method: UL 94, and thickness tested (mm): 0.8

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

500 V

Show Supplier Material materials with Comparative tracking index of 500 V

IEC 60112, Sol.A, DAM

Surface resistivity

23.0 °C

1.00E+12 Ω/sq

Show Supplier Material materials with Surface resistivity of 1.00E+12 Ω/sq

IEC 60093, 500V, DAM

Volume resistivity

23.0 °C

1.00E+14 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+14 Ω·cm

IEC 60093, 500V, DAM

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

1.4 %

Show Supplier Material materials with Shrinkage of 1.4 %

ISO 294-4, DAM

Shrinkage, transverse

23.0 °C

1.5 %

Show Supplier Material materials with Shrinkage, transverse of 1.5 %

ISO 294-4, DAM

Technological properties

Property
Certifications

RoHS 2011/65/UE

Color

Black

Fillers

30% Mineral Powder

Processing methods

Injection Molding